added amorphous si
Line 4: Line 4:
=[[PECVD 1 (PlasmaTherm 790)]]=
=[[PECVD 1 (PlasmaTherm 790)]]=


=== [https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1270764394 PECVD 1 Plots] ===
===[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1270764394 PECVD 1 Plots]===


==SiO<sub>2</sub> [PECVD 1]==
==SiO<sub>2</sub> [PECVD 1]==
Line 48: Line 48:
=[[PECVD 2 (Advanced Vacuum)]]=
=[[PECVD 2 (Advanced Vacuum)]]=


=== [https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=272916741 PECVD 2 Plots] ===
===[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=272916741 PECVD 2 Plots]===


==SiO<sub>2</sub> [PECVD 2]==
==SiO<sub>2</sub> [PECVD 2]==
Line 81: Line 81:
===Historical Data===
===Historical Data===
[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=268003895 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>]
[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=268003895 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data</nowiki>]
==Amorphous Silicone [PECVD 2]==

===Standard Recipe===
Amorphous Silicone [PECVD 2] Standard Recipe

===Present Data===
Amorphous Silicone [PECVD 2] Present Data

===Historical Data===
Amorphous Silicone [PECVD 2] Historical Data
==Standard Cleaning Procedure [PECVD 2]==
==Standard Cleaning Procedure [PECVD 2]==
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
Line 113: Line 123:
The system currently has Deuterated Silane (SiD<sub>4</sub>) installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.
The system currently has Deuterated Silane (SiD<sub>4</sub>) installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.


=== [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Plots] ===
===[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Plots]===


==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==
Line 166: Line 176:
=[[Ion Beam Deposition (Veeco NEXUS)]]=
=[[Ion Beam Deposition (Veeco NEXUS)]]=


=== [https://docs.google.com/spreadsheets/d/11A0ac8NU51bmcQ_grQcq9wuPwWnfy1_9MNk2DEo5yyo/edit#gid=2030038046 IBD Plots] ===
===[https://docs.google.com/spreadsheets/d/11A0ac8NU51bmcQ_grQcq9wuPwWnfy1_9MNk2DEo5yyo/edit#gid=2030038046 IBD Plots]===


==SiO<sub>2</sub> [IBD]==
==SiO<sub>2</sub> [IBD]==

Revision as of 20:09, 30 November 2021

Back to Vacuum Deposition Recipes

PECVD 1 (PlasmaTherm 790)

PECVD 1 Plots

SiO2 [PECVD 1]

Standard Recipe

SiO2 [PECVD 1] Standard Recipe

Present Data

SiO2 [PECVD 1] Present Data

Historical Data

SiO2 [PECVD 1] Historical Data

Si3N4 [PECVD 1]

Standard Recipe

Si3N4 [PECVD 1] Standard Recipe

Present Data

Si3N4 [PECVD 1] Present Data

Historical Data

Si3N4 [PECVD 1] Historical Data

Low Stress Si3N4 [PECVD 2]

Standard Recipe

Low Stress Si3N4 [PECVD 1] Standard Recipe

Present Data

Low Stress Si3N4 [PECVD 1] Present Data

Historical Data

Low Stress Si3N4 [PECVD 1] Historical Data

Standard Cleaning Procedure [PECVD 1]

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.

Standard Cleaning Recipe [CF4/O2 Clean]

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

PECVD 2 (Advanced Vacuum)

PECVD 2 Plots

SiO2 [PECVD 2]

Standard Recipe

SiO2 [PECVD 2] Standard Recipe

Present Data

SiO2 [PECVD 2] Present Data

Historical Data

SiO2 [PECVD 2] Historical Data

Si3N4 [PECVD 2]

Standard Recipe

Si3N4 [PECVD 2] Standard Recipe

Present Data

Si3N4 [PECVD 2] Present Data

Historical Data

Si3N4 [PECVD 2] Historical Data

Low Stress Si3N4 [PECVD 2]

Standard Recipe

Low Stress Si3N4 [PECVD 2] Standard Recipe

Present Data

Low Stress Si3N4 [PECVD 2] Present Data

Historical Data

Low Stress Si3N4 [PECVD 2] Historical Data

Amorphous Silicone [PECVD 2]

Standard Recipe

Amorphous Silicone [PECVD 2] Standard Recipe

Present Data

Amorphous Silicone [PECVD 2] Present Data

Historical Data

Amorphous Silicone [PECVD 2] Historical Data

Standard Cleaning Procedure [PECVD 2]

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. (If >29min dep time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again.
  2. Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.

Standard Clean Recipe [STD CF4/O2 Clean recipe]

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Clean Times (PECVD#2)

Film Deposited Cleaning Time (Dry)
SiO2 1 min. clean for every 1 min. deposition
Si3N4 1 min. clean for every 7 min of deposition
If > 29min total dep time

(Season + Dep)

Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

ICP-PECVD (Unaxis VLR)

2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.

ICP-PECVD Plots

Low Deposition Rate SiO2 [ICP-PECVD]

Standard Recipe

Low Deposition Rate SiO2 [ICP-PECVD] Standard Recipe

Present Data

Low Deposition Rate SiO2 [ICP-PECVD] Present Data

Historical Data

Low Deposition Rate SiO2 [ICP-PECVD] Historical Data

High Deposition Rate SiO2 [ICP-PECVD]

Standard Recipe

High Deposition Rate SiO2 [ICP-PECVD] Standard Recipe

Present Data

High Deposition Rate SiO2 [ICP-PECVD] Present Data

Historical Data

High Deposition Rate SiO2 [ICP-PECVD] Historical Data

Si3N4 [ICP-PECVD]

Standard Recipe

Si3N4 [ICP-PECVD] Standard Recipe

Present Data

Si3N4 [ICP-PECVD] Present Data

Historical Data

Si3N4 [ICP-PECVD] Historical Data

Low Stress Si3N4 [ICP-PECVD]

Standard Recipe

Low Stress Si3N4 [ICP-PECVD] Standard Recipe

Present Data

Low Stress Si3N4 [ICP-PECVD] Present Data

Historical Data

Low Stress Si3N4 [ICP-PECVD] Historical Data

Standard Cleaning Procedure [ICP-PECVD]

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min

Standard Clean Recipe

Ion Beam Deposition (Veeco NEXUS)

IBD Plots

SiO2 [IBD]

Standard Recipe

SiO2 [IBD] Standard Recipe

Present Data

SiO2 [IBD] Present Data

Historical Data

SiO2 [IBD] Historical Data

Si3N4 [IBD]

Standard Recipe

Si3N4 [IBD] Standard Recipe

Present Data

Si3N4 [IBD] Present Data

Historical Data

Si3N4 [IBD] Historical Data

Ta2O5 [IBD]

Standard Recipe

Ta2O5 [IBD] Standard Recipe

Present Data

Ta2O5 [IBD] Present Data

Historical Data

Ta2O5 [IBD] Historical Data

Al2O3 [IBD]

Standard Recipe

Al2O3 [IBD] Standard Recipe

Present Data

Al2O3 [IBD] Present Data

Historical Data

Al2O3 [IBD] Historical Data

TiO2 [IBD]

Standard Recipe

TiO2 [IBD] Standard Recipe

Present Data

TiO2 [IBD] Present Data

Historical Data

TiO2 [IBD] Historical Data

Standard Cleaning Procedure [ICP-PECVD]

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min

Standard Clean Recipe