Line 15: Line 15:
|1.2
|1.2
|82.1
|82.1
|[https://www.nanotech.ucsb.edu/wiki/index.php/File:SiO2_Etch_using_ICP2-no_O2.pdf]
|[https://www.nanotech.ucsb.edu/wiki/images/1/13/SiO2_Etch_using_ICP2-no_O2.pdf]
|-
|-
|1/28/2019
|1/28/2019

Revision as of 19:06, 31 January 2019

ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
10/5/2018 SiO2#02 160 1.2 82.1 [1]
1/28/2019 I21901 146 1.23 [2]