Line 13: Line 13:
|1.2
|1.2
|82.1
|82.1
|-
|1/28/2019
|I21901
|146
|1.2
|
|}
|}
[https://www.nanotech.ucsb.edu/wiki/index.php/File:SiO2_Etch_using_ICP2-no_O2.pdf File:SiO2 Etch using ICP2-no O2.pdf]
[https://www.nanotech.ucsb.edu/wiki/index.php/File:SiO2_Etch_using_ICP2-no_O2.pdf File:SiO2 Etch using ICP2-no O2.pdf]

Revision as of 17:16, 29 January 2019

ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o)
10/5/2018 SiO2#02 160 1.2 82.1
1/28/2019 I21901 146 1.2

File:SiO2 Etch using ICP2-no O2.pdf