Revision as of 16:06, 19 July 2019
ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec | |||||
Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) | SEM Images |
10/5/2018 | SiO2#02 | 160 | 1.2 | 82.1 | [1] |
1/28/2019 | I21901 | 146 | 1.23 | [2] | |
3/6/2019 | I21904 | 151 | 1.23 | 85.6 | https://www.nanotech.ucsb.edu/wiki/images/8/87/SiO2_Etch_using_ICP2_no_O2-3-06-2019.pdf |
7/18/2019 | I21905 | 162 | 1.37 |