RIE 2 (MRC): Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
added SOP link
No edit summary
Line 34: Line 34:


==Procedures==
==Procedures==
⚫
[https://signupmonkey.ece.ucsb.edu/wiki/images/4/4f/RIE_2_SOP.pdf RIE #2 Standard Operating Procedure]

⚫
* [https://signupmonkey.ece.ucsb.edu/wiki/images/4/4f/RIE_2_SOP.pdf RIE #2 Standard Operating Procedure]

Revision as of 22:03, 11 September 2019

RIE 2 (MRC)
Tool Type Dry Etch
Location Bay 2
Supervisor Lee Sawyer
Supervisor Phone (805) 893-2123
Supervisor E-Mail lee_sawyer@ucsb.edu
Description RIE #2 Methane/Hydrogen-Based System
Manufacturer Materials Research Corporation (MRC)
Dry Etch Recipes
Sign up for this tool


About

This is a Materials Research Corporation RIE-51 parallel plate, 13.56 Mhz system used primarily for the etching of InP with CH4/H2/Ar gases, although it can be used to etch As- and Sb-based III-V compounds and a variety of II-VI semiconductors as well. For Al-containing compounds and II-VI compounds, high bias power is required. Tool features include: six inch diameter water cooled cathode/substrate platform, pyrex cylinder for plasma confinement and gas flow control, adjustable cathode-anode spacing, fixed bias or power control and HeNe laser etch monitor with chart recorder. It is diffusion pumped and has no loadlock. Various etching applications have included: in-plane lasers/facets, InP-based HBTs, FET gate recessing, InP-based quantum microcavities, Bragg-Fresnel x-ray lenses and waveguides.

RIE of InP and related compounds can be achieved with a hydride-based process chemistry of methane/hydrogen with an etching mechanism due to a "reverse" metalorganic CVD reaction. Because both etching and deposition occur simultaneously, it is important to use the proper gas flows and to periodically remove any polymer reaction by-products deposited on the non-etched (mask) surfaces. (This system has an additional flow circuit in order to bleed in small amounts, <1 sccm, of O2). Alternatively, one can perform cyclic etching between MHA and O2 to keep polymer formation to a minimum. With this technique selectivity is quite high and anisotropic etching can be achieved. While a metal, dielectric or photoresist may be used as a mask, photoresist should only be used at low bias voltages in order to avoid mask pattern distortions due to reflow. A precoat etch should be done before etching to condition the chamber.

Detailed Specifications

  • Etch gases include: CH4, H2, Ar and O2
  • Low 1 E -6 ultimate chamber pressure
  • 13.56 Mhz excitation frequency
  • Sample size limited to approximately 2 inches
  • HeNe and IR laser monitoring for endpoint
  • Automatic tuning network
  • DC Bias or RF power control
  • Masking materials include: Ni, SiON, photoresist (limited to low bias/power)
  • Typical etch conditions for InGaAsP:
    • 75 mT (CH4/H2/Ar : 4/20/10 sccm)
    • 450v bias
    • ~ 45 nm/min. etch rate

Procedures