Test Data of etching SiO2 with CHF3/CF4: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
adding a pic |
Text replacement - "www.nanotech.ucsb.edu/wiki/" to "wiki.nanotech.ucsb.edu/wiki/" |
||
| Line 15: | Line 15: | ||
|1.2 |
|1.2 |
||
|82.1 |
|82.1 |
||
|[https:// |
|[https://wiki.nanotech.ucsb.edu/wiki/images/1/13/SiO2_Etch_using_ICP2-no_O2.pdf] |
||
|- |
|- |
||
|1/28/2019 |
|1/28/2019 |
||
| Line 22: | Line 22: | ||
|1.23 |
|1.23 |
||
| |
| |
||
|[https:// |
|[https://wiki.nanotech.ucsb.edu/wiki/images/f/f9/SiO2_Etch_using_ICP2-no_O2-a.pdf] |
||
|- |
|- |
||
|3/6/2019 |
|3/6/2019 |
||
| Line 29: | Line 29: | ||
|1.23 |
|1.23 |
||
|85.6 |
|85.6 |
||
|[https:// |
|[https://wiki.nanotech.ucsb.edu/wiki/images/8/87/SiO2_Etch_using_ICP2_no_O2-3-06-2019.pdf] |
||
|- |
|- |
||
|7/18/2019 |
|7/18/2019 |
||
| Line 36: | Line 36: | ||
|1.37 |
|1.37 |
||
| |
| |
||
|[https:// |
|[https://wiki.nanotech.ucsb.edu/wiki/images/2/23/I2190506.pdf] |
||
|- |
|- |
||
|1/16/2020 |
|1/16/2020 |
||
Revision as of 01:29, 7 April 2020
| ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec | |||||
| Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) | SEM Images |
| 10/5/2018 | SiO2#02 | 160 | 1.2 | 82.1 | [1] |
| 1/28/2019 | I21901 | 146 | 1.23 | [2] | |
| 3/6/2019 | I21904 | 151 | 1.23 | 85.6 | [3] |
| 7/18/2019 | I21905 | 162 | 1.37 | [4] | |
| 1/16/2020 | I22001 | 149 | 1.21 | [5] | |