Test Data of etching SiO2 with CHF3/CF4: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
add a SEM |
add a data point |
||
| Line 61: | Line 61: | ||
|5/19/2021 |
|5/19/2021 |
||
|I22102 |
|I22102 |
||
| |
|163 |
||
|1.11 |
|1.11 |
||
|Etch time=130 sec |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/4/4c/I2210214.pdf] |
|[https://wiki.nanotech.ucsb.edu/w/images/4/4c/I2210214.pdf] |
||
|} |
|} |
||
Revision as of 02:30, 20 May 2021
| ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec | |||||
| Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) | SEM Images |
| 10/5/2018 | SiO2#02 | 160 | 1.2 | 82.1 | [1] |
| 1/28/2019 | I21901 | 146 | 1.23 | [2] | |
| 3/6/2019 | I21904 | 151 | 1.23 | 85.6 | [3] |
| 7/18/2019 | I21905 | 162 | 1.37 | [4] | |
| 1/16/2020 | I22001 | 149 | 1.21 | [5] | |
| 8/9/2020 | I22002 | 102 | 0.86 | caused by air leaking to CHF3 channel | [6] |
| 1/7/2021 | I22101 | 144 | 1.20 | [7] | |
| 5/19/2021 | I22102 | 163 | 1.11 | Etch time=130 sec | [8] |