Revision as of 02:30, 10 August 2021
| ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec | |||||
| Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) | SEM Images |
| 10/5/2018 | SiO2#02 | 160 | 1.2 | 82.1 | [1] |
| 1/28/2019 | I21901 | 146 | 1.23 | [2] | |
| 3/6/2019 | I21904 | 151 | 1.23 | 85.6 | [3] |
| 7/18/2019 | I21905 | 162 | 1.37 | [4] | |
| 1/16/2020 | I22001 | 149 | 1.21 | [5] | |
| 8/9/2020 | I22002 | 102 | 0.86 | caused by air leaking to CHF3 channel | [6] |
| 1/7/2021 | I22101 | 144 | 1.20 | [7] | |
| 5/19/2021 | I22102 | 163 | 1.11 | Etch time=130 sec | [8] |
| 7/21/2021 | I22103 | 134 | 1.09 | Investigating reports of low etch rate | [9] |
| 8/9/2021 | I22105 | 140 | 0.97 | After etching diamond sample for 1 hour using Cl2/Ar | [10] |