InP Etch Rate and Selectivity (InP/SiO2)

From UCSB Nanofab Wiki
Revision as of 23:06, 20 April 2018 by Ningcao (talk | contribs) (Latest InP etch test result)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)
Jump to navigation Jump to search
1.4 mT, 125/800W, Cl2/H2/Ar flow-rate=6.3/12.7/2 sccm, chuck temperature=200 C, and etch time=90s (Prior to the etch, do O2 plasma chamber clean for 15 minutes, then, chamber coating with the same recipe and a quarter dummy InP on carrier
Date  InP Etch Rtae (mm/min) Selectivity (InP/SiO2)
4/10/2018 1.12 12.8