Test Data of etching SiO2 with CHF3/CF4
From UCSB Nanofab Wiki
Revision as of 19:06, 31 January 2019 by
Ningcao
(
talk
|
contribs
)
(add a SEM pic)
(
diff
)
← Older revision
|
Latest revision
(
diff
) |
Newer revision →
(
diff
)
Jump to navigation
Jump to search
ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
Date
Sample#
Etch Rate (nm/min)
Etch Selectivity (SiO2/PR)
Averaged Sidewall Angle (
o
)
SEM Images
10/5/2018
SiO2#02
160
1.2
82.1
[1]
1/28/2019
I21901
146
1.23
[2]
Navigation menu
Personal tools
Create account
Log in
Namespaces
Page
Discussion
English
Views
Read
View source
View history
More
Search
InvisibleMenu
QuickLinks
Lab Rules
Common Questions/FAQ
Staff List
Equipment Signup
Chemicals + MSDS
Protofab
Equipment
Full Tool List
Lithography
Vacuum Deposition
Dry Etch
Wet Processing
Thermal Processing
Packaging
Metrology & Test
Recipes and Data
Lithography
Vacuum Deposition
Dry Etching
Wet Etching
Thermal Processing
Packaging Tools
Data + Info
Process Control Data
Tutorials
Calculators/Utilities
NanoFab Info
Research + Pubs
Tech Talks
Tools
What links here
Related changes
Special pages
Printable version
Permanent link
Page information