ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
Date
Sample#
Etch Rate (nm/min)
Etch Selectivity (SiO2/PR)
Averaged Sidewall Angle (
o
)
SEM Images
10/5/2018
SiO2#02
160
1.2
82.1
[1]
1/28/2019
I21901
146
1.23
[2]
3/6/2019
I21904
151
1.23
85.6
Navigation menu
Personal tools
Create account
Log in
Namespaces
Page
Discussion
English
Views
Read
View source
View history
More
Search
InvisibleMenu
QuickLinks
Lab Rules
Common Questions/FAQ
Staff List
Equipment Signup
Chemicals + MSDS
Protofab
Equipment
Full Tool List
Lithography
Vacuum Deposition
Dry Etch
Wet Processing
Thermal Processing
Packaging
Metrology & Test
Recipes and Data
Lithography
Vacuum Deposition
Dry Etching
Wet Etching
Thermal Processing
Packaging Tools
Data + Info
Process Control Data
Tutorials
Calculators/Utilities
NanoFab Info
Research + Pubs
Tech Talks
Tools
What links here
Related changes
Special pages
Printable version
Permanent link
Page information