Florine ICP: 3.8mT, 50/800W, CHF3/CF4=10/30sccm, and Time=90 sec | |||||
Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) | SEM Images |
1/28/2021 | FE2102 | 309 | 0.99 | [1] |