Wet Etching Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
→Table of Wet Etching Recipes: added GaSb substrate removal etch
 
(55 intermediate revisions by 5 users not shown)
Line 1: Line 1:
__TOC__
== References ==
[http://ieeexplore.ieee.org/abstract/document/546406/ Etch rates for Micromachining Processing (IEEE Jnl. MEMS, 1996)] - includes tables of etch rates of numerous metals vs. various wet and dry etchants.


==Chemicals Available==
[http://ieeexplore.ieee.org/abstract/document/1257354/ Etch rates for micromachining-Part II (IEEE Jnl. MEMS, 2003)] - expanded tables containing resists, dielectrics, metals and semiconductors vs. many wet etch chemicals.


*[[Chemical List|'''The Chemical Lists''']] show stocked chemicals, photolithography chemicals, and how to bring new chemicals.
[http://www.sciencedirect.com/science/article/pii/S0927796X00000279 Guide to references on III±V semiconductor chemical etching] - exhaustive list of wet etchants for etching various semiconductors, including selective etches.

==Compound Semiconductor Etching==
[http://www.sciencedirect.com/science/article/pii/S0927796X00000279 Guide to references on III±V semiconductor chemical etching]

Please add any confirmed etches from this reference to the {{HLink|Wet Etching Recipes|The Master Table of Wet Etching (Include All Materials)}}. Thanks!

==Metal Etching==
*[[media:Ta and Cr E-beam deposition and wet etch test.pdf|Selective Wet Etch of Cr over Ta using Cr Etchant]]
*[[media:ITO Deposition-250C-Ebeam2-HCl-Wet-Etch.pdf|Wet Etch of ITO using Heated, Diluted HCl Solution]]

==Silicon etching==
[http://ieeexplore.ieee.org/xpls/abs_all.jsp?arnumber=546406 Etch rates for micromachining processing] Please add any confirmed etches from this reference to the Master Table of Wet Etching.

[http://ieeexplore.ieee.org/xpls/abs_all.jsp?arnumber=1257354 Etch rates for micromachining processing-part II] Please add any confirmed etches from this reference to the Master Table of Wet Etching.

==Dielectric etching==

==Organic removal==

==Gold Plating==

==Chemi-Mechanical Polishing (CMP)==


==Example Wet Etching Table==
How to use the Master Table of Wet Etching:

When entering a new etch into the table make a row for every etchant used in the solution such that the information can be sorted by etchant. For example, the InP etch HCl:H3PO4(1:3) and H3PO4:HCl(3:1). Likewise, if etch is known to be selective to multiple materials the etch should have a row for each material. For example HCl:H3PO4(1:3) is selective to both InGaAs and InGaAsP.

This multiple entry method may seem laborious for the person entering a new etch, however the power of sorting by selective materials and chemicals in a table with all materials is great.


=='''Table of Wet Etching Recipes'''==
''Use the ↑ ↓ Arrows in the header row to sort the entire table by material, selectivity, etchant etc.''
{| class="wikitable sortable"
{| class="wikitable sortable"
|-
|-
! Material !! Etchant !! Rate (nm/min) !! Anisotropy !! Selective to !! Selectivity !! Ref. !! Notes !! Confirmed by !! Extra column
!Material!!Etchant!!Rate (nm/min)!!Anisotropy!!Selective to!!Selectivity!!Ref.!!Notes!!Confirmed By/Date
|-
|-
|Photoresist, polymers/organics
| InP|| HCl:H3PO4(1:3)|| ~1000 || Highly || InGaAs || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
|H2SO4:H2O2 = 3:1
[[Wet Etching Recipes#Organic%20removal|Piranha Solution]]
|typ. 5-10min etch for polymer residue
|
|Cr, W, Au, Pt, Si, SiO2, SiN
|
|
|'''''Dangerous''''' boiling hazard - see '''''[[Wet Etching Recipes#Piranha%20Solution|Piranha Solution]]'''''
section below. Etches Ti, Ni, Hf
|[[Demis D. John]], 2017
|-
|-
|InP
| InP|| HCl:H3PO4(1:3)|| ~1000 || Highly || InGaAsP || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
|H3PO4:HCl = 3:1
|~1000
|Highly
|InGaAsP
|High
|[http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)]
|
|
|-
|-
| InP|| H3PO4:HCl(3:1)|| ~1000 || Highly || InGaAs || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
|InP||H3PO4:HCl = 3:1||~1000||Highly||InGaAs||High||[http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)]||
|
|-
|-
|InP
| InP|| H3PO4:HCl(3:1)|| ~1000 || Highly || InGaAsP || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
|HCl:H2O = 3:1
|}
|~5000
|
|InGaAs or InGaAsP
~200nm stop-etch
|High
|
|Bubbles while etching
|
|-
|InGaAs
|H2SO4:H2O2:H2O = 1:1:10
|~600
|
|InP
|High
|
|Exothermic, may reduce selectivity if hot
|
|-
|InGaAsP
|H2SO4:H2O2:H2O = 1:1:10
|~600
|
|InP
|High
|
|Exothermic, may reduce selectivity if hot
(same as InGaAs stop-etch removal)
|
|-
|GaAs
|NH4OH:H2O2 = 1:30
|
| -
|AlGaAs,
Al > 80%


~200nm stop-etch
==The Master Table of Wet Etching (Include '''All''' Materials)==
|High

|
{| class="wikitable sortable"
|
|Garrett Cole
|-
|-
|GaSb
! Material !! Etchant !! Rate (nm/min) !! Anisotropy !! Selective to !! Selectivity !! Ref. !! Notes !! Confirmed by !! Extra column
|[https://dtrinkle.matse.illinois.edu/MatSE584/kap_6/advanced/t6_1_2.html Sirtl etch]:
CrO3 powder mixed with HF
|TBD
|TBD
|InAs
|Infinite
|PhD. Dissertation of Shamsul Arafin, T.U. Munich.
|Do not store mixed - will corrode and leak out of the bottle! Mix fresh every time. Read MSDS's!
|
|-
|-
|AlGaAs,
| InP|| HCl:H3PO4(1:3)|| ~1000 || Highly || InGaAs || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
Al ≥80%
|HF:H2O = 1:20
|
| -
|GaAs
|High
|
|
|Garrett Cole
|-
|-
|Oxide of InP
| InP|| HCl:H3PO4(1:3)|| ~1000 || Highly || InGaAsP || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
|NH4OH:H2O = 1:10
|1min to remove
|
|InP
|unknown
|
|
|[[Ning Cao]]
|-
|-
|Oxide of GaAs
| InP|| H3PO4:HCl(3:1)|| ~1000 || Highly || InGaAs || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
|HCl:H2O = 1:10
|1min to remove
|
|GaAs
|unknown
|
|
|[[Demis D. John]]
|-
|-
|Al2O3 ''(ALD Plasma 300C)''||Developer: 300MIF||~1.6||None
| InP|| H3PO4:HCl(3:1)|| ~1000 || Highly || InGaAsP || High || [http://tel.archives-ouvertes.fr/docs/00/76/94/02/PDF/VA2_LAMPONI_MARCO_15032012.pdf Lamponi (p.102)] || Example || Jon Doe || Example
|Most non-Al Materials.
|High||Measured in-house||Rate slows with time.||JTB
|-
|-
|Al2O3 ''(ALD Plasma 300C)''||Developer: 400K||~2.2||None
| Al2O3 (ALD Plasma 300C)|| 300MIF || ~1.6 || || || High || Measured in-house || Rate slows with time, Selective to most non-Al Materials || JTB || Example
|Most non-Al Materials.
|High||Measured in-house||Rate slows with time.||JTB
|-
|-
| Al2O3 (ALD Plasma 300C)|| 400K || ~2.2 || || || High || Measured in-house || Rate slows with time, Selective to most non-Al Materials || JTB || Example
|Al2O3 ''(ALD Plasma 300C)''||Developer: 400K (1:4)||~1.6||None
|Most non-Al Materials.
|High||Measured in-house||Rate slows with time.||JTB
|-
|-
| Al2O3 (ALD Plasma 300C)|| 400K(1:4) || ~1.6 || || || High || Measured in-house || Rate slows with time, Selective to most non-Al Materials || JTB || Example
|Al2O3 ''(ALD Plasma 300C)''||NH4OH:H2O2:H2O (1:2:50)||~<0.5|| || || ||Measured in-house||Rate slows with time||JTB
|-
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Al2O3_deposition_.28IBD.29 Al2O3 ''(IBD)'']
| Al2O3 (ALD Plasma 300C)|| NH4OH:H2O2:H2O (1:2:50) || ~<0.5 || || || High || Measured in-house || Rate slows with time || JTB || Example
|HF ("Buffered HF Improved", Transene)
|~170
|None
|Photoresist
|High
|Measured in-house
|May need to increase adhesion with thin SiO2 layer, and 100°C baked HMDS.
|Biljana Stamenic,
2017-12
|-
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Al2O3_deposition_.28IBD.29 Al2O3 ''(IBD)'']
| Al2O3 (ALD Plasma 300C)|| H2O2:NH4OH:H2O (2:1:50) || ~<0.5 || || || High || Measured in-house || Rate slows with time || JTB || Example
|Developer: 726 MiF
|3.5
|None
|Most non-Al Materials.
|High
|Measured in-house
|
|Demis D. John,
2017-11
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Al2O3_Deposition_.28Sputter_4.29 Al2O3 ''(AJA#4)'']
|Developer: 300 MiF
|4.30
|None
|Most non-Al Materials.
|High
|Measured in-house
|
|Demis D. John
2018-02
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#SiO2_deposition_.28PECVD_.231.29 SiO2 ''(PECVD #1)'']
|HF ("Buffered HF Improved", Transene)
|~550
|None
|Photoresist
|High
|Measured in-house
|May need to increase adhesion with 100°C baked HMDS.
|Biljana Stamenic
2023
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#SiO2_deposition_.28PECVD_.232.29 SiO2 ''(PECVD #2)'']
|HF ("Buffered HF Improved", Transene)
|~680
|None
|Photoresist
|High
|Measured in-house
|May need to increase adhesion with 100°C baked HMDS.
|Biljana Stamenic
2023
|-
|SiO2 ''(ALD -BDEAS 300C)''
|HF ("Buffered")
Diluted with DI
BHF:H2O = 1:100
|~7.46
|
|
|
|Measured in-house
|
|Biljana Stamenic
2024
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#SiO2_deposition_.28IBD.29 SiO2 (IBD)]
|HF ("Buffered HF Improved", Transene)
|~260
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanofab.ucsb.edu/wiki/PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29 SiO2 LDR ''(Unaxis VLR)'']
|HF ("Buffered HF Improved", Transene)
|~170
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanofab.ucsb.edu/wiki/PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29 SiO2 HDR ''(Unaxis VLR)'']
|HF ("Buffered HF Improved", Transene)
|~230
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#SiN_deposition_.28PECVD_.231.29 Si3N4 (PECVD#1)]
|HF ("Buffered HF Improved", Transene)
|~120
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#SiN_deposition_.28PECVD_.232.29 Si3N4 (PECVD#2)]
|HF ("Buffered HF Improved", Transene)
|~35
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Low-Stress_SiN_deposition_.28PECVD_.232.29 Si3N4 Low-Stress (PECVD#2)]
|HF ("Buffered HF Improved", Transene)
|~30
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Si3N4_deposition_.28IBD.29 Si3N4 (IBD)]
|HF ("Buffered HF Improved", Transene)
|~5
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanofab.ucsb.edu/wiki/PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29 SiN ''(Unaxis VLR)'']
|HF ("Buffered HF Improved", Transene)
|~10
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanofab.ucsb.edu/wiki/PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29 SiN Low Stress ''(Unaxis VLR)'']
|HF ("Buffered HF Improved", Transene)
|~135
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Ta2O5_deposition_.28IBD.29 Ta2O5 (IBD)]
|HF ("Buffered HF Improved", Transene)
|0.07
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2023
|-
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#TiO2_deposition_.28IBD.29 TiO2 (IBD)]
|HF ("Buffered HF Improved", Transene)
|1.0–2.0
|None
|Photoresist
|High
|Measured in-house
|
|Biljana Stamenic
2014-12
|-
|Si (<100> crystalline)
|KOH (45%) @ 87°C
|~730
|High, Crystallographic, ~55°
|Low-Stress Si3N4 - either [[PECVD Recipes#Low-Stress SiN deposition .28PECVD .232.29|PECVD #2]] or Commercial LPCVD Si3N4
Other Si3N4 also OK.
|LS-SiN: High
PR etches quickly, SiO2 etches slowly.
|Measured In-House
- Search online.
|Use the Covered, Heated vertical bath ([[Wet Benches#Wafer Toxic Corrosive Benches|Dedi cated bath in Bay 4]]). Slight Bubbler.
|Brian Thibeault
2017
|-
!Material!!Etchant!!Rate (nm/min)!!Anisotropy!!Selective to!!Selectivity!!Ref.!!Notes!!Confirmed By/Date
|}
|}


==Wet Etching References==

#[http://ieeexplore.ieee.org/abstract/document/546406/ Etch rates for Micromachining Processing (IEEE Jnl. MEMS, 1996)] - includes tables of etch rates of numerous metals vs. various wet and dry etchants.
#[http://ieeexplore.ieee.org/abstract/document/1257354/ Etch rates for micromachining-Part II (IEEE Jnl. MEMS, 2003)] - expanded tables containing resists, dielectrics, metals and semiconductors vs. many wet etch chemicals.
#[http://www.sciencedirect.com/science/article/pii/S0927796X00000279 Guide to references on III±V semiconductor chemical etching] - exhaustive list of wet etchants for etching various semiconductors, including selective etches.
#[http://transene.com/etch-compatibility/ Transene's Chemical Compatibility Chart] provides a useful quick-reference for which Transene etchants attack which materials.
##As a side-note, [http://transene.com/ Transene] provides many pre-mixed solutions that you can order, saving you the time and uncertainty of measuring/mixing such chemicals yourself. Make sure you check with us before ordering so we know how to handle the chemical before it arrives.

===Compound Semiconductor Etching===
[http://www.sciencedirect.com/science/article/pii/S0927796X00000279 Guide to references on III±V semiconductor chemical etching (A.R. Clawson, 2001)]

* Impressively vast list of various III-V wet etches, organized by various applications (eg. "selective GaAs against AlGaAs" or "non-selective InP/InGaAsP" etc.)
* Please add any confirmed etches from this reference to the {{HLink|Wet Etching Recipes|The Master Table of Wet Etching (Include All Materials)}}.

===Metal Etching===

*[//wiki.nanotech.ucsb.edu/w/images/c/c3/Ta_and_Cr_E-beam_deposition_and_wet_etch_test.pdf Selective Wet Etch of Cr over Ta using Cr Etchant]
*[//wiki.nanotech.ucsb.edu/w/images/d/dc/ITO_Deposition-250C-Ebeam2-HCl-Wet-Etch.pdf Wet Etch of ITO using Heated, Diluted HCl Solution]

===Silicon etching===
[http://ieeexplore.ieee.org/xpls/abs_all.jsp?arnumber=546406 Etch rates for micromachining processing]

[http://ieeexplore.ieee.org/xpls/abs_all.jsp?arnumber=1257354 Etch rates for micromachining processing-part II]

Please add any confirmed etches from this reference to the {{HLink|Wet Etching Recipes|The Master Table of Wet Etching (Include All Materials)}}.

==Organic removal==

===Piranha Solution===

*'''Careful!''' Read about how to prepare and handle this safely:
**[http://web.mit.edu/cortiz/www/PiranhaSafety.doc MIT's Piranha Solution safety document]
**[https://www.ehs.harvard.edu/sites/default/files/lab_safety_guideline_piranha_etch.pdf Harvard EHS's Handling Document]
**Used for etching away Photoresist residues after dry etching.

===PureStrip (Transene)===

*Heat to @ 70°C
**[[Wet Benches#Wafer Toxic Corrosive Benches|Vertical heated bath on Wafer Toxic-Corrosive bench in Bay 4]]
**After a few days heated, it loses potency - must drain + replenish with fresh solution.
**~30-90min will remove stubborn, microscopic PR residues from dry etching.

==[[Gold Plating Bench|Gold Plating Bench (Technic SEMCON 1000)]]==
Standard plating recipes are described and taught during the equipment training for this tool.

Electroplating first requires a Gold seed layer to be present on all surfaces to be plated. Common ways to produce this are to:

*[[Tool List#Sputter Deposition|Sputter-coat]] a thin (~100nm) Au "seed layer" on all surfaces of the wafer, being careful to consider shadowing effects during the dep (eg. in high-aspect ratio trenches).
*Perform photolithography to protect (and prevent plating) in desired areas - areas with no photoresist will be plated.
**Leave ''Open'' the 4 contact points on the edge of the wafer, or some other contact point, for an electrode to make contact to the Seed layer.
**Optionally use EBR100 to swab away photoresist from the contact points.
*Perform the electroplating on the [[Gold Plating Bench|Technic SemCon]], contacting the seed layer with electrodes and executing the program for the desired current/time to achieve the plating thickness (typically microns).
*Strip the photoresist using standard solvents.
*Use the [[CAIBE (Oxford Ion Mill)|Oxford Ion Mill]] to blanket etch the seed layer all over the wafer (the 100nm removed from the plated regions will be negligible compared to the ~1µm plated).

==[[Chemical-Mechanical Polisher (Logitech)|Chemi-Mechanical Polishing (CMP)]]==
''To Be Added''

==[[Mechanical Polisher (Allied)|Mechanical Polishing (Allied)]]==
''To Be Added''
[[Category:Processing]]
[[Category:Processing]]

Latest revision as of 03:25, 5 September 2026

Chemicals Available

  • The Chemical Lists show stocked chemicals, photolithography chemicals, and how to bring new chemicals.

Table of Wet Etching Recipes

Use the ↑ ↓ Arrows in the header row to sort the entire table by material, selectivity, etchant etc.

Material Etchant Rate (nm/min) Anisotropy Selective to Selectivity Ref. Notes Confirmed By/Date
Photoresist, polymers/organics H2SO4:H2O2 = 3:1

Piranha Solution

typ. 5-10min etch for polymer residue Cr, W, Au, Pt, Si, SiO2, SiN Dangerous boiling hazard - see Piranha Solution

section below. Etches Ti, Ni, Hf

Demis D. John, 2017
InP H3PO4:HCl = 3:1 ~1000 Highly InGaAsP High Lamponi (p.102)
InP H3PO4:HCl = 3:1 ~1000 Highly InGaAs High Lamponi (p.102)
InP HCl:H2O = 3:1 ~5000 InGaAs or InGaAsP

~200nm stop-etch

High Bubbles while etching
InGaAs H2SO4:H2O2:H2O = 1:1:10 ~600 InP High Exothermic, may reduce selectivity if hot
InGaAsP H2SO4:H2O2:H2O = 1:1:10 ~600 InP High Exothermic, may reduce selectivity if hot

(same as InGaAs stop-etch removal)

GaAs NH4OH:H2O2 = 1:30 - AlGaAs,

Al > 80%

~200nm stop-etch

High Garrett Cole
GaSb Sirtl etch:

CrO3 powder mixed with HF

TBD TBD InAs Infinite PhD. Dissertation of Shamsul Arafin, T.U. Munich. Do not store mixed - will corrode and leak out of the bottle! Mix fresh every time. Read MSDS's!
AlGaAs,

Al ≥80%

HF:H2O = 1:20 - GaAs High Garrett Cole
Oxide of InP NH4OH:H2O = 1:10 1min to remove InP unknown Ning Cao
Oxide of GaAs HCl:H2O = 1:10 1min to remove GaAs unknown Demis D. John
Al2O3 (ALD Plasma 300C) Developer: 300MIF ~1.6 None Most non-Al Materials. High Measured in-house Rate slows with time. JTB
Al2O3 (ALD Plasma 300C) Developer: 400K ~2.2 None Most non-Al Materials. High Measured in-house Rate slows with time. JTB
Al2O3 (ALD Plasma 300C) Developer: 400K (1:4) ~1.6 None Most non-Al Materials. High Measured in-house Rate slows with time. JTB
Al2O3 (ALD Plasma 300C) NH4OH:H2O2:H2O (1:2:50) ~<0.5 Measured in-house Rate slows with time JTB
Al2O3 (IBD) HF ("Buffered HF Improved", Transene) ~170 None Photoresist High Measured in-house May need to increase adhesion with thin SiO2 layer, and 100°C baked HMDS. Biljana Stamenic,

2017-12

Al2O3 (IBD) Developer: 726 MiF 3.5 None Most non-Al Materials. High Measured in-house Demis D. John,

2017-11

Al2O3 (AJA#4) Developer: 300 MiF 4.30 None Most non-Al Materials. High Measured in-house Demis D. John

2018-02

SiO2 (PECVD #1) HF ("Buffered HF Improved", Transene) ~550 None Photoresist High Measured in-house May need to increase adhesion with 100°C baked HMDS. Biljana Stamenic

2023

SiO2 (PECVD #2) HF ("Buffered HF Improved", Transene) ~680 None Photoresist High Measured in-house May need to increase adhesion with 100°C baked HMDS. Biljana Stamenic

2023

SiO2 (ALD -BDEAS 300C) HF ("Buffered")

Diluted with DI BHF:H2O = 1:100

~7.46 Measured in-house Biljana Stamenic

2024

SiO2 (IBD) HF ("Buffered HF Improved", Transene) ~260 None Photoresist High Measured in-house Biljana Stamenic

2023

SiO2 LDR (Unaxis VLR) HF ("Buffered HF Improved", Transene) ~170 None Photoresist High Measured in-house Biljana Stamenic

2023

SiO2 HDR (Unaxis VLR) HF ("Buffered HF Improved", Transene) ~230 None Photoresist High Measured in-house Biljana Stamenic

2023

Si3N4 (PECVD#1) HF ("Buffered HF Improved", Transene) ~120 None Photoresist High Measured in-house Biljana Stamenic

2023

Si3N4 (PECVD#2) HF ("Buffered HF Improved", Transene) ~35 None Photoresist High Measured in-house Biljana Stamenic

2023

Si3N4 Low-Stress (PECVD#2) HF ("Buffered HF Improved", Transene) ~30 None Photoresist High Measured in-house Biljana Stamenic

2023

Si3N4 (IBD) HF ("Buffered HF Improved", Transene) ~5 None Photoresist High Measured in-house Biljana Stamenic

2023

SiN (Unaxis VLR) HF ("Buffered HF Improved", Transene) ~10 None Photoresist High Measured in-house Biljana Stamenic

2023

SiN Low Stress (Unaxis VLR) HF ("Buffered HF Improved", Transene) ~135 None Photoresist High Measured in-house Biljana Stamenic

2023

Ta2O5 (IBD) HF ("Buffered HF Improved", Transene) 0.07 None Photoresist High Measured in-house Biljana Stamenic

2023

TiO2 (IBD) HF ("Buffered HF Improved", Transene) 1.0–2.0 None Photoresist High Measured in-house Biljana Stamenic

2014-12

Si (<100> crystalline) KOH (45%) @ 87°C ~730 High, Crystallographic, ~55° Low-Stress Si3N4 - either PECVD #2 or Commercial LPCVD Si3N4

Other Si3N4 also OK.

LS-SiN: High

PR etches quickly, SiO2 etches slowly.

Measured In-House

- Search online.

Use the Covered, Heated vertical bath (Dedi cated bath in Bay 4). Slight Bubbler. Brian Thibeault

2017

Material Etchant Rate (nm/min) Anisotropy Selective to Selectivity Ref. Notes Confirmed By/Date

Wet Etching References

  1. Etch rates for Micromachining Processing (IEEE Jnl. MEMS, 1996) - includes tables of etch rates of numerous metals vs. various wet and dry etchants.
  2. Etch rates for micromachining-Part II (IEEE Jnl. MEMS, 2003) - expanded tables containing resists, dielectrics, metals and semiconductors vs. many wet etch chemicals.
  3. Guide to references on III±V semiconductor chemical etching - exhaustive list of wet etchants for etching various semiconductors, including selective etches.
  4. Transene's Chemical Compatibility Chart provides a useful quick-reference for which Transene etchants attack which materials.
    1. As a side-note, Transene provides many pre-mixed solutions that you can order, saving you the time and uncertainty of measuring/mixing such chemicals yourself. Make sure you check with us before ordering so we know how to handle the chemical before it arrives.

Compound Semiconductor Etching

Guide to references on III±V semiconductor chemical etching (A.R. Clawson, 2001)

  • Impressively vast list of various III-V wet etches, organized by various applications (eg. "selective GaAs against AlGaAs" or "non-selective InP/InGaAsP" etc.)
  • Please add any confirmed etches from this reference to the The Master Table of Wet Etching (Include All Materials).

Metal Etching

Silicon etching

Etch rates for micromachining processing

Etch rates for micromachining processing-part II

Please add any confirmed etches from this reference to the The Master Table of Wet Etching (Include All Materials).

Organic removal

Piranha Solution

PureStrip (Transene)

Gold Plating Bench (Technic SEMCON 1000)

Standard plating recipes are described and taught during the equipment training for this tool.

Electroplating first requires a Gold seed layer to be present on all surfaces to be plated. Common ways to produce this are to:

  • Sputter-coat a thin (~100nm) Au "seed layer" on all surfaces of the wafer, being careful to consider shadowing effects during the dep (eg. in high-aspect ratio trenches).
  • Perform photolithography to protect (and prevent plating) in desired areas - areas with no photoresist will be plated.
    • Leave Open the 4 contact points on the edge of the wafer, or some other contact point, for an electrode to make contact to the Seed layer.
    • Optionally use EBR100 to swab away photoresist from the contact points.
  • Perform the electroplating on the Technic SemCon, contacting the seed layer with electrodes and executing the program for the desired current/time to achieve the plating thickness (typically microns).
  • Strip the photoresist using standard solvents.
  • Use the Oxford Ion Mill to blanket etch the seed layer all over the wafer (the 100nm removed from the plated regions will be negligible compared to the ~1µm plated).

Chemi-Mechanical Polishing (CMP)

To Be Added

Mechanical Polishing (Allied)

To Be Added