Microscope-mounted Optical Thin-Film Analyzer
Microscope-mounted Optical Thin-Film Analyzer
=== Startup and Calibration ===
=== Startup and Calibration ===
# Turn on light source to about 12 o'clock [[File:Filmetrics F40-UV - light source setting 02.jpg|thumb|150x150px|Set the light source to 12 o'clock]]
# Turn on light source to about 12 o'clock
## Optionally wait a few min for light intensity to stabilize.
## Optionally wait 1 min for light intensity to stabilize.[[File:Filmetrics F40-UV - light source setting 02.jpg|thumb|150x150px|Set the light source to 12 o'clock|none]]
# Open Software "'''FILMeasure'''". Activate "'''Live Video'''" Tab.
# Open Software "'''FILMeasure'''".
# Activate the "'''Live Video'''" Tab.
# Load "Filmetrics Focus/Reference Wafer" onto stage, avoiding hole [[File:Filmetrics F40-UV - wafer placement 03.jpg|thumb|200x200px|Approximate placement of a 4-inch wafer]]
# Load "'''''Filmetrics Focus / Reference Wafer'''''" onto stage, avoiding hole [[File:Filmetrics F40-UV - wafer placement 03.jpg|thumb|200x200px|Approximate placement of a 4-inch wafer|none]]
# Rotate uScope turret to desired microscope objective
# Rotate uScope turret to desired microscope objective
# Focus on wafer - use edge of blue (SiO2) features
# Focus on wafer - use edge of blue (SiO2) features
# In "'''Live Video'''" tab, make sure wafer is in focus, and black spot (measurement region) is on grey Silicon region only.
# In "'''Live Video'''" tab, make sure wafer is in focus, and black spot (measurement region) is on grey Silicon region only.[[File:Filmetrics F40-UV - focus on bare silicon 04.jpg|thumb|200x200px|Focus on the bare silicon in the FILMeasure software, for Si Reference scan|alt="Live Video" tab showing focused wafer|none]]
# Set software to use appropriate Objective calibration from dropdown list, eg. "10x"
# Set software to use appropriate Objective calibration from dropdown list, eg. "10x"[[File:Filmetrics F40-UV - objective choice 05.jpg|thumb|200x200px|Choose objective calibration in software|none]]
# Click '''[Baseline…]''', set to "'''Si'''" and '''[Take Reflectance Standard]''' & '''[Next-->]'''
# Click '''[Baseline…]''', set to "'''Si'''" and '''[Take Reflectance Standard]''' & '''[Next-->]'''
## If a warning about intensity change pops up, ignore it and hit '''[OK]'''
## If a warning about intensity change pops up, ignore it and hit '''[OK]'''
# Move stage so microscope shoots through hole in stage
# Move stage so microscope shoots through hole in stage
⚫
# Click '''[Take Background]''' & '''[Finish]'''[[File:Filmetrics F40-UV - dark meas thru hole 06.jpg|alt=microscope aiming through hole in stage|thumb|200x200px|For Background measurement, aim the microscope through the hole in the stage.|none]]
# Click '''[Take Background]''' & '''[Finish]'''
{|
![[File:Filmetrics F40-UV - focus on bare silicon 04.jpg|thumb|200x200px|Focus on the bare silicon in the FILMeasure software, for Si Reference scan|alt="Live Video" tab showing focused wafer]]
![[File:Filmetrics F40-UV - objective choice 05.jpg|thumb|200x200px|Choose objective calibration in software]]
⚫
![[File:Filmetrics F40-UV - dark meas thru hole 06.jpg|alt=microscope aiming through hole in stage|thumb|200x200px|For Background measurement, aim the microscope through the hole in the stage.]]
|}

=== Sample Measurement ===
=== Sample Measurement ===
# Focus on your sample/feature of interest & place the black aperture spot on the measurement region. Here we will measure the SiO<sub>2</sub> on the Filmetrics Reference Wafer.
# Focus on your sample/feature of interest & place the black aperture spot on the measurement region. Here we will measure the SiO<sub>2</sub> on the Filmetrics Reference Wafer.
## It is ok to change the objective, just make sure same calibrated objective is chosen before measuring.
## It is ok to change the objective, just make sure the same calibrated objective is chosen before measuring.
# Select a recipe from the Dropdown list (ok to ''discard changes''), and Click '''[Edit Recipe…]''' to set the layers to approximately what you expect to measure.
# Select a recipe from the Dropdown list (ok to ''discard changes''), and Click '''[Edit Recipe…]''' to set the layers to approximately what you expect to measure.
## Enable the checkbox next to the thicknesses you want it to measure/calculate, and Disable checkboxes next to any values you want the software to use pre-programmed values for.
## Enable the checkbox next to the thicknesses you want it to measure/calculate, and Disable checkboxes next to any values you want the software to use pre-programmed values for.
## Optionally enable the check box next to n & k - but only if you know what refractive index and extinction you expect.  If you don't know these values, Disable the "Meas" checkbox for n & k.  When enabled, you'll want to make sure the refractive index (n) is close to the expected value.
## Optionally enable the check box next to '''n''' & '''k''' - but only if you know what refractive index and extinction you expect.  If you don't know these values, Disable the "Meas" checkbox for n & k.  When enabled, you'll want to make sure the calculated refractive index (n) is close to the expected value.
# '''Re-Select the correct microscope objective''' & Click '''[Measure]'''
# '''Re-Select the correct microscope objective''' & Click '''[Measure]'''
# Make sure the blue (measured) and red (calc'd) curves have reasonably good agreement.  Goodness of fit >90% is pretty good.  Refractive Index (n), if calc'd, should be near the expected value for the film.
# Make sure the blue (measured) and red (calc'd) curves have reasonably good agreement.  Goodness of fit >90% is pretty good.  Refractive Index (n), if calc'd, should be near the expected value for the film.
## If fit is bad (low GOF) or refractive index is far off, this measurement is inaccurate.  If Red curve is much too wavy or too smooth, then your guess of thickness was not close enough - '''[Edit Recipe]''' & '''[Analyze]''' again until you get a good fit. [[File:Filmetrics F40-UV - spectrum curve fit 07.jpg|alt=example spectrum curve fit|none|thumb|300x300px|A good fit should show the Calculated (red) curve overlay on top of the Measureed (blue) curve.]]
## If fit is bad (low GoF) or refractive index is far off, this measurement is inaccurate.  If Red curve is much too wavy or too smooth, then your guess of thickness was not close enough - '''[Edit Recipe]''' & '''[Analyze]''' again until you get a good fit.
## Don't hesitate to ask [[Ning Cao|Ning]] or [[Demis D. John|Demis]] for help with the curve-fitting, it can be complicated!
:: [[File:Filmetrics F40-UV - spectrum curve fit 07.jpg|alt=example spectrum curve fit|none|thumb|300x300px|A good fit should show the Calculated (red) curve overlay on top of the Measureed (blue) curve.]]


=== ShutDown ===
=== ShutDown ===

Latest revision as of 18:13, 31 May 2019

Demis D. John, UCSB NanoFab, Updated: 2018-07-17

Microscope-mounted Optical Thin-Film Analyzer

Startup and Calibration

  1. Turn on light source to about 12 o'clock
    1. Optionally wait 1 min for light intensity to stabilize.
      Set the light source to 12 o'clock
  2. Open Software "FILMeasure".
  3. Activate the "Live Video" Tab.
  4. Load "Filmetrics Focus / Reference Wafer" onto stage, avoiding hole
    Approximate placement of a 4-inch wafer
  5. Rotate uScope turret to desired microscope objective
  6. Focus on wafer - use edge of blue (SiO2) features
  7. In "Live Video" tab, make sure wafer is in focus, and black spot (measurement region) is on grey Silicon region only.
    "Live Video" tab showing focused wafer
    Focus on the bare silicon in the FILMeasure software, for Si Reference scan
  8. Set software to use appropriate Objective calibration from dropdown list, eg. "10x"
    Choose objective calibration in software
  9. Click [Baseline…], set to "Si" and [Take Reflectance Standard] & [Next-->]
    1. If a warning about intensity change pops up, ignore it and hit [OK]
  10. Move stage so microscope shoots through hole in stage
  11. Click [Take Background] & [Finish]
    microscope aiming through hole in stage
    For Background measurement, aim the microscope through the hole in the stage.

Sample Measurement

  1. Focus on your sample/feature of interest & place the black aperture spot on the measurement region. Here we will measure the SiO2 on the Filmetrics Reference Wafer.
    1. It is ok to change the objective, just make sure the same calibrated objective is chosen before measuring.
  2. Select a recipe from the Dropdown list (ok to discard changes), and Click [Edit Recipe…] to set the layers to approximately what you expect to measure.
    1. Enable the checkbox next to the thicknesses you want it to measure/calculate, and Disable checkboxes next to any values you want the software to use pre-programmed values for.
    2. Optionally enable the check box next to n & k - but only if you know what refractive index and extinction you expect.  If you don't know these values, Disable the "Meas" checkbox for n & k.  When enabled, you'll want to make sure the calculated refractive index (n) is close to the expected value.
  3. Re-Select the correct microscope objective & Click [Measure]
  4. Make sure the blue (measured) and red (calc'd) curves have reasonably good agreement.  Goodness of fit >90% is pretty good.  Refractive Index (n), if calc'd, should be near the expected value for the film.
    1. If fit is bad (low GoF) or refractive index is far off, this measurement is inaccurate.  If Red curve is much too wavy or too smooth, then your guess of thickness was not close enough - [Edit Recipe] & [Analyze] again until you get a good fit.
    2. Don't hesitate to ask Ning or Demis for help with the curve-fitting, it can be complicated!
example spectrum curve fit
A good fit should show the Calculated (red) curve overlay on top of the Measureed (blue) curve.

ShutDown

  1. Set objective to 10x & Remove Sample
  2. TURN OFF THE LIGHT SOURCE
    1. The halogen light source does die eventually, so prolong the life by turning off when not in use.
    2. If doing repeated measurements, leave a note with date/time.