===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)===
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)===


*Recipe name: '''''Ch3_TMA+H2O-300C'''''
*Recipe name: '''''CH3-TMA+H2O-<u>300C</u>'''''
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc
**300°C Dep., Water reaction
**300°C Dep., Water reaction
**This is considered the standard recipe for ALD
*Recipe Name: CH3_TMA+H2O-XYZ?
**Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
**TBD
*Recipe Name: '''''CH3-TMA+250W/O*-300C'''''
**Similar deposition rate
**Oxygen Plasma reaction instead of H2O
**Lower carbon content, faster depsition.
**Temperature variations: 300°C (std.), 200°C, 120°C
*Recipe Name: '''''CH3-TMA+O3/200mT-300C'''''
**Similar dep. rate
**Ozone (O<sub>3</sub>) reactant, experimental


===AlN deposition (ALD CHAMBER 3)===
===AlN deposition (ALD CHAMBER 3)===
*Recipe name: '''''Ch3_TMA+100W/20N*-300C'''''
*Recipe name: '''''CH3-TMA+100W/N*-300C'''''
**AlN deposition rate ~ t.b.d.
**AlN deposition rate ~ t.b.d.
**Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
**Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
**300°C Dep.
**Temperature Variations: 300°C Dep. (std.), 200*C, 120°C
**Power variations: 300W, 400W (at 300°C)
**Nitrogen/Hydrogen variations: "30N*/30H*" at 200*C and 300°C


===HfO{{sub|2}} deposition (ALD CHAMBER 3)===
===HfO{{sub|2}} deposition (ALD CHAMBER 3)===
*Recipe name: '''''Ch3_TEMAH+H2O-300C'''''
*Recipe name: '''''CH3-TEMAH+H2O-300C'''''
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
**300°C Dep.
*Recipe name: '''''CH3-TEMAH+250W/O*-300C'''''
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O
*Recipe name: '''''CH3-TEMAH+O3/100mT-300C'''''
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O


===SiO{{sub|2}} deposition (ALD CHAMBER 3)===
===SiO{{sub|2}} deposition (ALD CHAMBER 3)===
*Recipe name: '''''Ch3_TDMAS+250W/O*-300C'''''
*Recipe name: '''''CH3-TDMAS+250W/O*-300C'''''
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
**Temperature variations: 300*C (std.), 250°C, 230°C, 200°C, 150°C, 120°C
*Recipe name: '''''CH3-TDMAS+O3/200mT-300C'''''
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O


===ZrO{{sub|2}} deposition (ALD CHAMBER 3)===
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)===
*Recipe name: '''''Ch3_TEMAZ+H2O-300C'''''
*Recipe name: '''''CH3-TEMAZ+H2O-300C'''''
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above.
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above.
**300°C Dep.
**Temperature variations: 300°C (std.), 200°C
*Recipe name: '''''CH3-TEMAZ+250W/O*-300C'''''
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O
*Recipe name: '''''CH3-TEMAZ+O3/100mT-300C'''''
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O


===TiO{{sub|2}} deposition (ALD CHAMBER 3)===
===TiO{{sub|2}} deposition (ALD CHAMBER 3)===
*Recipe name: '''''Ch3_TDMAT+H2O-300C'''''
*Recipe name: '''''CH3-TDMAT+H2O-300C'''''
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Temperature variations: 300°C (std.), 200°C, 120*C
**300°C Dep.
*Recipe name: '''''CH3-TDMAT+250W/O*-300C'''''
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O


===TiN deposition (ALD CHAMBER 3)===
===TiN deposition (ALD CHAMBER 3)===
*Recipe name: '''''Ch3_TDMAT+N*/H*-300C'''''
*Recipe name: '''''CH3-TDMAT+400W/12N*/4H*-300C'''''
**TiN deposition rate ~ 0.7A/cyc
**TiN deposition rate ~ 0.7A/cyc
**Conductivity data: (to be added)
**Conductivity data: (to be added)
**300°C Dep, uses Plasma of N2 & H2 gases.
**Uses Plasma of N2 & H2 gases.
**Temperatures: 300°C (std.), 200°C
*Recipe name: '''''CH3-TDMAT+100W/N*-300C'''''
**Uses Plasma of N2 only
**Temperatures: 300°C (std.), 200°C
*Recipe name: '''''CH3-TDMAT+100W/NH3*-300C'''''
**Uses Plasma of NH<sub>3</sub> only
**Temperatures: 300°C (std.), 200°C

Revision as of 17:12, 15 May 2020

Back to Vacuum Deposition Recipes.

Atomic Layer Deposition (Oxford FlexAL)

Oxford FlexAL Chamber #1: Metals

Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)

Pt deposition (ALD CHAMBER 1)

  • Recipe name: Ch1_TMCpPt+O3-300C
  • Pt deposition rate ~ 0.5-0.6 A/cyc
  • Conductivity data: (to be added)
  • recipe utilizes the ozone generator which must be first set to the following conditions:
    • O2 flow = 250sccm
    • O3 concentration = 15 wt%
  • 300°C Deposition

Ru deposition (ALD CHAMBER 1)

  • Recipe name: Ch1_Ex03Ru[HPbub]+O2-300C
  • Ru deposition rate ~ 0.6-0.7A/cyc.
  • Conductivity data: (to be added)
  • 300°C, O2 gas reaction

ZnO Deposition (ALD Chamber 1)

Conductive film.

  • Recipe name: Ch1_DEZ+H2O-200C
  • ZnO deposition rate ≈ 1.6 A/cycle
  • resistivity ≈ TBA
  • 200°C Deposition, Water reaction

ZnO:Al deposition (ALD CHAMBER 1)

Al-Doped ZnO for variable resisitivity.

  • Recipe name: Ch1_DEZ/TMA+H2O-200C
    • The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.
  • Al dose fraction = 5% for lowest resistivity
  • ZnO deposition rate ~ 1.7A/cyc
  • resistivity ~ 4200uOhm.cm (390A film)

Oxford FlexAL Chamber #3: Dielectrics

Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)

Al2O3 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TMA+H2O-300C
    • Al2O3 deposition rate ~ 1A/cyc
    • 300°C Dep., Water reaction
    • This is considered the standard recipe for ALD
    • Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
  • Recipe Name: CH3-TMA+250W/O*-300C
    • Similar deposition rate
    • Oxygen Plasma reaction instead of H2O
    • Lower carbon content, faster depsition.
    • Temperature variations: 300°C (std.), 200°C, 120°C
  • Recipe Name: CH3-TMA+O3/200mT-300C
    • Similar dep. rate
    • Ozone (O3) reactant, experimental

AlN deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TMA+100W/N*-300C
    • AlN deposition rate ~ t.b.d.
    • Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
    • Temperature Variations: 300°C Dep. (std.), 200*C, 120°C
    • Power variations: 300W, 400W (at 300°C)
    • Nitrogen/Hydrogen variations: "30N*/30H*" at 200*C and 300°C

HfO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TEMAH+H2O-300C
    • HfO2 deposition rate ~ 0.9-1.0A/cyc
    • Note: deposition shows significant parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
    • Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
  • Recipe name: CH3-TEMAH+250W/O*-300C
    • Uses Oxygen plasma reactant instead of H2O
  • Recipe name: CH3-TEMAH+O3/100mT-300C
    • Uses Ozone (O3) for reactant instead of H2O

SiO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TDMAS+250W/O*-300C
    • SiO2 deposition rate ~ 0.7-0.8A/cyc
    • Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
    • Temperature variations: 300*C (std.), 250°C, 230°C, 200°C, 150°C, 120°C
  • Recipe name: CH3-TDMAS+O3/200mT-300C
    • Uses Ozone (O3) for reactant instead of H2O

ZrO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TEMAZ+H2O-300C
    • ZrO2 deposition rate ~ 0.9-1.0A/cyc
    • Not directly characterized since results are basically the same as the HfO2 process above.
    • Temperature variations: 300°C (std.), 200°C
  • Recipe name: CH3-TEMAZ+250W/O*-300C
    • Uses Oxygen plasma reactant instead of H2O
  • Recipe name: CH3-TEMAZ+O3/100mT-300C
    • Uses Ozone (O3) for reactant instead of H2O

TiO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TDMAT+H2O-300C
    • TiO2 deposition rate ~ 0.6A/cyc
    • Note: deposition shows parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
    • Temperature variations: 300°C (std.), 200°C, 120*C
  • Recipe name: CH3-TDMAT+250W/O*-300C
    • Uses Oxygen plasma reactant instead of H2O

TiN deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TDMAT+400W/12N*/4H*-300C
    • TiN deposition rate ~ 0.7A/cyc
    • Conductivity data: (to be added)
    • Uses Plasma of N2 & H2 gases.
    • Temperatures: 300°C (std.), 200°C
  • Recipe name: CH3-TDMAT+100W/N*-300C
    • Uses Plasma of N2 only
    • Temperatures: 300°C (std.), 200°C
  • Recipe name: CH3-TDMAT+100W/NH3*-300C
    • Uses Plasma of NH3 only
    • Temperatures: 300°C (std.), 200°C