Atomic Layer Deposition Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Atomic Layer Deposition (Oxford FlexAL): Recipe info on Plasma, Ratios
Al2O3 deposition (ALD CHAMBER 3): added terms "Plasma/Thermal/Ozone". Also added Chamber 1 Al2O3
Line 2: Line 2:
=[[Atomic Layer Deposition (Oxford FlexAL)]]=
=[[Atomic Layer Deposition (Oxford FlexAL)]]=


== Oxford FlexAL Process Notes ==
==Oxford FlexAL Process Notes==


=== Temperature ===
===Temperature===
''To Be Added: effect of varying temeprature''
''To Be Added: effect of varying temeprature''


=== Plasma ===
===Plasma===
'''''O*''''' or '''''N*''''' mean Oxygen/Nitrogen plasma, respectively.
'''''O*''''' or '''''N*''''' mean Oxygen/Nitrogen plasma, respectively.


Line 14: Line 14:
The drawback is that the plasma shutter, which opens/closes between plasma steps, gets coated in materials and can cause higher particle counts.
The drawback is that the plasma shutter, which opens/closes between plasma steps, gets coated in materials and can cause higher particle counts.


=== Ozone ===
===Ozone===
'''''O3''''' indicates a recipe using the Ozone generator for reaction.
'''''O3''''' indicates a recipe using the Ozone generator for reaction.


''More info to be added''
''More info to be added''


=== Varying Atomic Ratios ===
===Varying Atomic Ratios===
For some recipes such as TiN, there are two loops in the recipe. The outermost loop controls the total thickness of the film, the inner loop controls the ratio between the two elements. Contact the superviosr for more detailed info.
For some recipes such as TiN, there are two loops in the recipe. The outermost loop controls the total thickness of the film, the inner loop controls the ratio between the two elements. Contact the superviosr for more detailed info.


== Oxford FlexAL Chamber #1: Metals ==
==Oxford FlexAL Chamber #1: Metals==
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.)
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.)

=== Pt deposition (ALD CHAMBER 1) ===
=== Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 1) ===

* Recipe name: '''''CH3-TMA+H2O-<u>300C</u>''''' ("Thermal")
**300°C Dep., Thermal Water reaction
**This is considered the standard recipe for ALD
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc
**Recipe variations: ''TBD''

===Pt deposition (ALD CHAMBER 1)===

*Recipe name: '''''Ch1_TMCpPt+O3-300C'''''
*Recipe name: '''''Ch1_TMCpPt+O3-300C'''''
**Pt deposition rate ~ 0.5-0.6 A/cyc
**Pt deposition rate ~ 0.5-0.6 A/cyc
Line 36: Line 46:
**300°C deposition
**300°C deposition


=== Ru deposition (ALD CHAMBER 1) ===
===Ru deposition (ALD CHAMBER 1)===
* Recipe name: '''''Ch1_Ex03Ru[HPbub]+O2-300C'''''
* Ru deposition rate ~ 0.6-0.7A/cyc.
* Conductivity data: (to be added)
* 300°C, O2 gas reaction


*Recipe name: '''''Ch1_Ex03Ru[HPbub]+O2-300C'''''
=== ZnO Deposition (ALD Chamber 1) ===
*Ru deposition rate ~ 0.6-0.7A/cyc.
*Conductivity data: (to be added)
*300°C, O2 gas reaction

===ZnO Deposition (ALD Chamber 1)===
''Conductive film.''
''Conductive film.''

* Recipe name: '''''Ch1_DEZ+H2O-200C'''''
*Recipe name: '''''Ch1_DEZ+H2O-200C'''''
* ZnO deposition rate ≈ 1.6 A/cycle
*ZnO deposition rate ≈ 1.6 A/cycle
*resistivity ≈ ''TBA''
*resistivity ≈ ''TBA''
*200°C Deposition, Water reaction
*200°C Deposition, Water reaction


=== ZnO:Al deposition (ALD CHAMBER 1) ===
===ZnO:Al deposition (ALD CHAMBER 1)===
''Al-Doped ZnO for variable resisitivity.''
''Al-Doped ZnO for variable resisitivity.''

*Recipe name: '''''Ch1_DEZ/TMA+H2O-200C'''''
*Recipe name: '''''Ch1_DEZ/TMA+H2O-200C'''''
**''The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.''
**''The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.''
*Al dose fraction = 5% for lowest resistivity
*Al dose fraction = 5% for lowest resistivity
*ZnO deposition rate ~ 1.7A/cyc
*ZnO deposition rate ~ 1.7A/cyc
*resistivity ~ 4200uOhm.cm (390A film)
*resistivity ~ 4200uOhm.cm (390A film)


== Oxford FlexAL Chamber #3: Dielectrics ==
==Oxford FlexAL Chamber #3: Dielectrics==
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.)
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.)


===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)===
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)===


*Recipe name: '''''CH3-TMA+H2O-<u>300C</u>'''''
*Recipe name: '''''CH3-TMA+H2O-<u>300C</u>''''' ("Thermal")
**300°C Dep., Thermal Water reaction
**This is considered the standard recipe for ALD
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc
**Temperature variations: 300°C (std.), '''250°C, 200°C, 150°C, 120°C'''
**300°C Dep., Water reaction
*Recipe Name: '''''CH3-TMA+250W/O*-300C''''' ("Plasma")
**This is considered the standard recipe for ALD
**Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
*Recipe Name: '''''CH3-TMA+250W/O*-300C'''''
**Similar deposition rate
**Oxygen Plasma reaction instead of H2O
**Oxygen Plasma reaction instead of H2O
**Lower carbon content, approx. <u>1.5–2x faster deposition rate.</u>
**Lower carbon content
**Approx. <u>1.5–2x faster deposition rate</u> than thermal.
**Temperature variations: 300°C (std.), 200°C, 120°C
**Temperature variations: 300°C (std.), '''200°C, 120°C'''
*Recipe Name: '''''CH3-TMA+O3/200mT-300C'''''
*Recipe Name: '''''CH3-TMA+O3/200mT-300C''''' ("Ozone")
**Similar dep. rate
**Similar dep. rate
**Ozone (O<sub>3</sub>) reactant, experimental
**Ozone (O<sub>3</sub>) reactant, experimental
**Requires Ozone generator to be turned on - ask supervisor


===AlN deposition (ALD CHAMBER 3)===
===AlN deposition (ALD CHAMBER 3)===

*Recipe name: '''''CH3-TMA+100W/N*-300C'''''
*Recipe name: '''''CH3-TMA+100W/N*-300C'''''
**AlN deposition rate ~ t.b.d.
**AlN deposition rate ~ t.b.d.
Line 85: Line 100:


===HfO{{sub|2}} deposition (ALD CHAMBER 3)===
===HfO{{sub|2}} deposition (ALD CHAMBER 3)===

*Recipe name: '''''CH3-TEMAH+H2O-300C'''''
*Recipe name: '''''CH3-TEMAH+H2O-300C''''' ("Thermal")
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
**Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
*Recipe name: '''''CH3-TEMAH+250W/O*-300C'''''
*Recipe name: '''''CH3-TEMAH+250W/O*-300C''''' ("Plasma")
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O
*Recipe name: '''''CH3-TEMAH+O3/100mT-300C'''''
*Recipe name: '''''CH3-TEMAH+O3/100mT-300C''''' ("Ozone")
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O
**Requires Ozone generator to be turned on - ask supervisor


===SiO{{sub|2}} deposition (ALD CHAMBER 3)===
===SiO{{sub|2}} deposition (ALD CHAMBER 3)===

*Recipe name: '''''CH3-TDMAS+250W/O*-300C'''''
*Recipe name: '''''CH3-TDMAS+250W/O*-300C''''' ("Plasma")
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
**Temperature variations: 300*C (std.), 250°C, 230°C, 200°C, 150°C, 120°C
**Temperature variations: 300*C (std.), 250°C, 230°C, 200°C, 150°C, 120°C
*Recipe name: '''''CH3-TDMAS+O3/200mT-300C'''''
*Recipe name: '''''CH3-TDMAS+O3/200mT-300C''''' ("Ozone")
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O
**Requires Ozone generator to be turned on - ask supervisor


===ZrO{{sub|2}} deposition (ALD CHAMBER 3)===
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)===

*Recipe name: '''''CH3-TEMAZ+H2O-300C'''''
*Recipe name: '''''CH3-TEMAZ+H2O-300C''''' ("Thermal")
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above.
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above.
**Temperature variations: 300°C (std.), 200°C
**Temperature variations: 300°C (std.), 200°C
*Recipe name: '''''CH3-TEMAZ+250W/O*-300C'''''
*Recipe name: '''''CH3-TEMAZ+250W/O*-300C''''' ("Plasma")
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O
*Recipe name: '''''CH3-TEMAZ+O3/100mT-300C'''''
*Recipe name: '''''CH3-TEMAZ+O3/100mT-300C''''' ("Ozone")
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O
**Requires Ozone generator to be turned on - ask supervisor


===TiO{{sub|2}} deposition (ALD CHAMBER 3)===
===TiO{{sub|2}} deposition (ALD CHAMBER 3)===

*Recipe name: '''''CH3-TDMAT+H2O-300C'''''
*Recipe name: '''''CH3-TDMAT+H2O-300C''''' ("Thermal")
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient.
**Temperature variations: 300°C (std.), 200°C, 120*C
**Temperature variations: 300°C (std.), 200°C, 120*C
*Recipe name: '''''CH3-TDMAT+250W/O*-300C'''''
*Recipe name: '''''CH3-TDMAT+250W/O*-300C''''' ("Plasma")
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O


===TiN deposition (ALD CHAMBER 3)===
===TiN deposition (ALD CHAMBER 3)===

*Recipe name: '''''CH3-TDMAT+400W/12N*/4H*-300C'''''
*Recipe name: '''''CH3-TDMAT+400W/12N*/4H*-300C'''''
**TiN deposition rate ~ 0.7A/cyc
**TiN deposition rate ~ 0.7A/cyc
Line 133: Line 156:
**Temperatures: 300°C (std.), 200°C
**Temperatures: 300°C (std.), 200°C


=== Historical Data (ALD Chamber 3) ===
===Historical Data (ALD Chamber 3)===

* [[Tbd|2021 ALD Al2O3 (H2O, 300°C) Historical Data]]
*[[Tbd|2021 ALD Al2O3 (H2O, 300°C) Historical Data]]

Revision as of 17:53, 21 January 2022

Back to Vacuum Deposition Recipes.

Atomic Layer Deposition (Oxford FlexAL)

Oxford FlexAL Process Notes

Temperature

To Be Added: effect of varying temeprature

Plasma

O* or N* mean Oxygen/Nitrogen plasma, respectively.

The plasma processes on this tool will run considerably faster than purely thermal proceses, because the reaction time is faster. Also, the O* plasma may reduce carbon contaminants from the organic precursors.

The drawback is that the plasma shutter, which opens/closes between plasma steps, gets coated in materials and can cause higher particle counts.

Ozone

O3 indicates a recipe using the Ozone generator for reaction.

More info to be added

Varying Atomic Ratios

For some recipes such as TiN, there are two loops in the recipe. The outermost loop controls the total thickness of the film, the inner loop controls the ratio between the two elements. Contact the superviosr for more detailed info.

Oxford FlexAL Chamber #1: Metals

Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)

Al2O3 deposition (ALD CHAMBER 1)

  • Recipe name: CH3-TMA+H2O-300C ("Thermal")
    • 300°C Dep., Thermal Water reaction
    • This is considered the standard recipe for ALD
    • Al2O3 deposition rate ~ 1A/cyc
    • Recipe variations: TBD

Pt deposition (ALD CHAMBER 1)

  • Recipe name: Ch1_TMCpPt+O3-300C
    • Pt deposition rate ~ 0.5-0.6 A/cyc
    • Conductivity data: (to be added)
    • recipe utilizes the ozone generator which must be first set to the following conditions:
      • O2 flow = 250sccm
      • O3 concentration = 15 wt%
    • 300°C deposition
  • Recipe name: CH1-TMCpPt+250W/O*-300C
    • Uses Oxygen plasma
    • 300°C deposition

Ru deposition (ALD CHAMBER 1)

  • Recipe name: Ch1_Ex03Ru[HPbub]+O2-300C
  • Ru deposition rate ~ 0.6-0.7A/cyc.
  • Conductivity data: (to be added)
  • 300°C, O2 gas reaction

ZnO Deposition (ALD Chamber 1)

Conductive film.

  • Recipe name: Ch1_DEZ+H2O-200C
  • ZnO deposition rate ≈ 1.6 A/cycle
  • resistivity ≈ TBA
  • 200°C Deposition, Water reaction

ZnO:Al deposition (ALD CHAMBER 1)

Al-Doped ZnO for variable resisitivity.

  • Recipe name: Ch1_DEZ/TMA+H2O-200C
    • The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.
  • Al dose fraction = 5% for lowest resistivity
  • ZnO deposition rate ~ 1.7A/cyc
  • resistivity ~ 4200uOhm.cm (390A film)

Oxford FlexAL Chamber #3: Dielectrics

Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)

Al2O3 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TMA+H2O-300C ("Thermal")
    • 300°C Dep., Thermal Water reaction
    • This is considered the standard recipe for ALD
    • Al2O3 deposition rate ~ 1A/cyc
    • Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
  • Recipe Name: CH3-TMA+250W/O*-300C ("Plasma")
    • Oxygen Plasma reaction instead of H2O
    • Lower carbon content
    • Approx. 1.5–2x faster deposition rate than thermal.
    • Temperature variations: 300°C (std.), 200°C, 120°C
  • Recipe Name: CH3-TMA+O3/200mT-300C ("Ozone")
    • Similar dep. rate
    • Ozone (O3) reactant, experimental
    • Requires Ozone generator to be turned on - ask supervisor

AlN deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TMA+100W/N*-300C
    • AlN deposition rate ~ t.b.d.
    • Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
    • Temperature Variations: 300°C Dep. (std.), 200*C, 120°C
    • Power variations: 300W, 400W (at 300°C)
    • Nitrogen/Hydrogen variations: "30N*/30H*" at 200*C and 300°C

HfO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TEMAH+H2O-300C ("Thermal")
    • HfO2 deposition rate ~ 0.9-1.0A/cyc
    • Note: deposition shows significant parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
    • Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
  • Recipe name: CH3-TEMAH+250W/O*-300C ("Plasma")
    • Uses Oxygen plasma reactant instead of H2O
  • Recipe name: CH3-TEMAH+O3/100mT-300C ("Ozone")
    • Uses Ozone (O3) for reactant instead of H2O
    • Requires Ozone generator to be turned on - ask supervisor

SiO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TDMAS+250W/O*-300C ("Plasma")
    • SiO2 deposition rate ~ 0.7-0.8A/cyc
    • Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
    • Temperature variations: 300*C (std.), 250°C, 230°C, 200°C, 150°C, 120°C
  • Recipe name: CH3-TDMAS+O3/200mT-300C ("Ozone")
    • Uses Ozone (O3) for reactant instead of H2O
    • Requires Ozone generator to be turned on - ask supervisor

ZrO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TEMAZ+H2O-300C ("Thermal")
    • ZrO2 deposition rate ~ 0.9-1.0A/cyc
    • Not directly characterized since results are basically the same as the HfO2 process above.
    • Temperature variations: 300°C (std.), 200°C
  • Recipe name: CH3-TEMAZ+250W/O*-300C ("Plasma")
    • Uses Oxygen plasma reactant instead of H2O
  • Recipe name: CH3-TEMAZ+O3/100mT-300C ("Ozone")
    • Uses Ozone (O3) for reactant instead of H2O
    • Requires Ozone generator to be turned on - ask supervisor

TiO2 deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TDMAT+H2O-300C ("Thermal")
    • TiO2 deposition rate ~ 0.6A/cyc
    • Note: deposition shows parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
    • Temperature variations: 300°C (std.), 200°C, 120*C
  • Recipe name: CH3-TDMAT+250W/O*-300C ("Plasma")
    • Uses Oxygen plasma reactant instead of H2O

TiN deposition (ALD CHAMBER 3)

  • Recipe name: CH3-TDMAT+400W/12N*/4H*-300C
    • TiN deposition rate ~ 0.7A/cyc
    • Conductivity data: (to be added)
    • Uses Plasma of N2 & H2 gases.
    • Temperatures: 300°C (std.), 200°C
  • Recipe name: CH3-TDMAT+100W/N*-300C
    • Uses Plasma of N2 only
    • Temperatures: 300°C (std.), 200°C
  • Recipe name: CH3-TDMAT+100W/NH3*-300C
    • Uses Plasma of NH3 only
    • Temperatures: 300°C (std.), 200°C

Historical Data (ALD Chamber 3)