Created page with "{| class="wikitable" | colspan="5" |ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec |- |Date |Sample# |Etch Rate (nm/min) |Etch Selectivity (SiO2/PR) |Averaged..."
 
Ningcao (talk | contribs)
No edit summary
Line 14:
|77.9
|}
https://www.nanotech.ucsb.edu/wiki/images/f/f1/SiO2_Etch_using_ICP2_with_O2.pdf

Revision as of 15:28, 9 October 2018

ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o)
10/5/2018 SiO2#01 95.2 0.74 77.9

https://www.nanotech.ucsb.edu/wiki/images/f/f1/SiO2_Etch_using_ICP2_with_O2.pdf