*Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc |
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc |
||
*Recipe Name: CH3_TMA+H2O-XYZ? |
|||
**TBD |
|||
===AlN deposition (ALD CHAMBER 3)=== |
===AlN deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''Ch3_TMA+100W/20N*-300C''''' |
*Recipe name: '''''Ch3_TMA+100W/20N*-300C''''' |
||
*AlN deposition rate ~ t.b.d. |
**AlN deposition rate ~ t.b.d. |
||
* |
**Recipe utilizes a N* plasma @ 100W, 20mTorr pressure. |
||
===HfO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===HfO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''Ch3_TEMAH+H2O-300C''''' |
*Recipe name: '''''Ch3_TEMAH+H2O-300C''''' |
||
*HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
||
*Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
||
===SiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===SiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''Ch3_TDMAS+250W/O*-300C''''' |
*Recipe name: '''''Ch3_TDMAS+250W/O*-300C''''' |
||
*SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc |
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc |
||
* |
**Recipe utilizes an O* plasma @ 250W, 5mTorr pressure |
||
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''Ch3_TEMAZ+H2O-300C''''' |
*Recipe name: '''''Ch3_TEMAZ+H2O-300C''''' |
||
*ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
||
* |
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above. |
||
===TiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===TiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''Ch3_TDMAT+H2O-300C''''' |
*Recipe name: '''''Ch3_TDMAT+H2O-300C''''' |
||
*TiO |
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc |
||
*Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
||
===TiN deposition (ALD CHAMBER 3)=== |
===TiN deposition (ALD CHAMBER 3)=== |
||
*Recipe name: '''''Ch3_TDMAT+N*/H*-300C''''' |
*Recipe name: '''''Ch3_TDMAT+N*/H*-300C''''' |
||
*TiN deposition rate ~ 0.7A/cyc |
**TiN deposition rate ~ 0.7A/cyc |
||
*Conductivity data: (to be added |
**Conductivity data: (to be added) |
Revision as of 00:33, 17 October 2018
Back to Vacuum Deposition Recipes.
Atomic Layer Deposition (Oxford FlexAL)
Oxford FlexAL Chamber #1: Metals
Pt deposition (ALD CHAMBER 1)
- Recipe name: Ch1_TMCpPt+O3-300C
- Pt deposition rate ~ 0.5-0.6A/cyc
- recipe utilizes the ozone generator which must be first set to the following conditions:
- O2 flow = 250sccm
- O3 concentration = 15 wt%
- Conductivity data: (to be added)
Ru deposition (ALD CHAMBER 1)
- Recipe name: Ch1_Ex03Ru[HPbub]+O2-300C
- Ru deposition rate ~ 0.6-0.7A/cyc.
- Conductivity data: (to be added)
ZnO Deposition (ALD Chamber 1)
Conductive film.
- Recipe name: Ch1_DEZ+H2O-200C
- ZnO deposition rate ≈ TBA
- resistivity ≈ TBA
ZnO:Al deposition (ALD CHAMBER 1)
Al-Doped ZnO for variable resisitivity.
- Recipe name: Ch1_DEZ/TMA+H2O-200C
- The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.
- Al dose fraction = 5% for lowest resistivity
- ZnO deposition rate ~ 1.7A/cyc
- resistivity ~ 4200uOhm.cm (390A film)
Oxford FlexAL Chamber #3: Dielectrics
Al2O3 deposition (ALD CHAMBER 3)
- Recipe name: Ch3_TMA+H2O-300C
- Al2O3 deposition rate ~ 1A/cyc
- Recipe Name: CH3_TMA+H2O-XYZ?
- TBD
AlN deposition (ALD CHAMBER 3)
- Recipe name: Ch3_TMA+100W/20N*-300C
- AlN deposition rate ~ t.b.d.
- Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
HfO2 deposition (ALD CHAMBER 3)
- Recipe name: Ch3_TEMAH+H2O-300C
- HfO2 deposition rate ~ 0.9-1.0A/cyc
- Note: deposition shows significant parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
SiO2 deposition (ALD CHAMBER 3)
- Recipe name: Ch3_TDMAS+250W/O*-300C
- SiO2 deposition rate ~ 0.7-0.8A/cyc
- Recipe utilizes an O* plasma @ 250W, 5mTorr pressure
ZrO2 deposition (ALD CHAMBER 3)
- Recipe name: Ch3_TEMAZ+H2O-300C
- ZrO2 deposition rate ~ 0.9-1.0A/cyc
- Not directly characterized since results are basically the same as the HfO2 process above.
TiO2 deposition (ALD CHAMBER 3)
- Recipe name: Ch3_TDMAT+H2O-300C
- TiO2 deposition rate ~ 0.6A/cyc
- Note: deposition shows parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
TiN deposition (ALD CHAMBER 3)
- Recipe name: Ch3_TDMAT+N*/H*-300C
- TiN deposition rate ~ 0.7A/cyc