Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer): Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Ningcao (talk | contribs)
add a SEM pic
Ningcao (talk | contribs)
add data
Line 23: Line 23:
|
|
|[https://www.nanotech.ucsb.edu/wiki/images/f/fa/SiO2_Etch_using_ICP2_with_O2-a.pdf]
|[https://www.nanotech.ucsb.edu/wiki/images/f/fa/SiO2_Etch_using_ICP2_with_O2-a.pdf]
|-
|3/6/2019
|I21903
|88.5
|0.80
|79.4
|
|}
|}

Revision as of 23:34, 6 March 2019

ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
10/5/2018 SiO2#01 95.2 0.74 77.9 [1]
1/28/2019 I21902 92.1 0.77 [2]
3/6/2019 I21903 88.5 0.80 79.4