Laser Etch Monitoring: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
m John d moved page Intellemetrics Laser Etch Monitoring to Laser Etch Monitoring without leaving a redirect: make it generic to all laser etch monitors
→Procedures: general procedure
Line 9: Line 9:


== Procedures ==
== Procedures ==

=== General Procedure ===
The basic method for performing an etch with laser monitoring endpoint, is as follows:
# Simulate or estimate what the laser monitor trace will look like, decide when to stop the etch according to the laser monitor plot.
# Mount the sample such that the laser will be able to reach a region to monitor the etch - typically ~100-300µm wide area.
# Load sample into chamber - wafer transfer '''only''', no etch.
# Align Laser onto area to monitor using co-axial microscope.
# Start laser power monitoring/logging.
# Start Etch (time set longer than expected etch time) - etch only, no wafer transfers.
## Closely observe laser monitor plot, comparing to known/simulated plot.
# Use "Next Step" or "End Step" when appropriate laser monitor trace is reached. Wait for process to complete any final steps.
# Transfer wafer out of chamber.
# Save laser monitor data, turn off laser & microscope illumination.

=== Specific Procedures ===
Procedures for specific machines are found on the following pages:
* [[Intellemetrics Laser Etch Monitor Procedure for Panasonic ICP Etchers]]
* [[Intellemetrics Laser Etch Monitor Procedure for Panasonic ICP Etchers]]
* [[Intellemetrics Laser Etch Monitor Procedure for Plasma-Therm Etchers]]
* [[Intellemetrics Laser Etch Monitor Procedure for Plasma-Therm Etchers]]

Revision as of 07:00, 15 May 2019

Overview

A number of our dry etching systems have Intellemetrics LEP500 Laser Etch monitors installed, for "endpoint detection". These systems allow you to end your etch at a known etch depth, or within a certain layer (with some caveats). This nearly eliminates the need to calibrate etch rates or to use timed etching only, which is especially important in our lab where etch rates can vary depending on the previous etches performed in the chamber.

Laser Etch monitoring works similarly to optical thin-film measurement via reflectivity spectra (eg. like our Filmetrics systems). However, instead of varying the optical wavelength and measuring a fixed thin-film, we measure a constant wavelength and a thin-film that is varying as it is etched. Thus, similar to the thin-film measurements, you can only measure a useful signal when the optical properties (reflection or interference) change during your etch.

For example, Etching from high-reflectivity Aluminum to Lower reflectivity Silicon will usually give you a clear drop showing that your Aluminum has been fully etched-through.

Etching films that are transparent at the laser monitor wavelength (670nm) produces a sinusoidal signal due to optical wave interference which gives you numerous possible stopping points to end the etch upon.

Procedures

General Procedure

The basic method for performing an etch with laser monitoring endpoint, is as follows:

  1. Simulate or estimate what the laser monitor trace will look like, decide when to stop the etch according to the laser monitor plot.
  2. Mount the sample such that the laser will be able to reach a region to monitor the etch - typically ~100-300µm wide area.
  3. Load sample into chamber - wafer transfer only, no etch.
  4. Align Laser onto area to monitor using co-axial microscope.
  5. Start laser power monitoring/logging.
  6. Start Etch (time set longer than expected etch time) - etch only, no wafer transfers.
    1. Closely observe laser monitor plot, comparing to known/simulated plot.
  7. Use "Next Step" or "End Step" when appropriate laser monitor trace is reached. Wait for process to complete any final steps.
  8. Transfer wafer out of chamber.
  9. Save laser monitor data, turn off laser & microscope illumination.

Specific Procedures

Procedures for specific machines are found on the following pages:

References

See the following pages for more information about laser endpoint detection.