Direct-Write Lithography Recipes: Difference between revisions
m updated THMR thickness |
added notes/comments to each section |
||
| Line 1: | Line 1: | ||
[[category: Lithography]] |
[[category: Lithography]] |
||
[[category: Recipes]] |
[[category: Recipes]] |
||
{{WIP}} |
|||
__TOC__ |
__TOC__ |
||
== [[Maskless Aligner (Heidelberg MLA150)]] == |
== [[Maskless Aligner (Heidelberg MLA150)]] == |
||
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. |
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point. |
||
These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches. |
|||
=== Positive Resist (MLA150) === |
=== Positive Resist (MLA150) === |
||
''We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work.'' |
|||
''General notes: Hotplates used, filters, laser wavelengths, etc.'' |
|||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
||
| Line 95: | Line 96: | ||
|AZ300MiF |
|AZ300MiF |
||
|20s |
|20s |
||
|line/space: |
|~0.4nm line/space: |
||
lower dose for clear-field, higher dose for dark-field. |
|||
|} |
|} |
||
=== Negative Resist (MLA150) === |
=== Negative Resist (MLA150) === |
||
''We found that all the negative PR's we tested required the 375nm in order to be fully exposure with reasonable dose.'' |
|||
''General notes: Hotplates used, filters, laser wavelengths, etc.'' |
|||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
||
| Line 159: | Line 160: | ||
=== Greyscale Lithography (MLA150) === |
=== Greyscale Lithography (MLA150) === |
||
''AZ4620 is the manufacturer-recommended PR for greyscale litho.'' |
|||
''Description...'' |
|||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
||
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
Revision as of 01:02, 14 November 2020
Maskless Aligner (Heidelberg MLA150)
Photolithography Recipes for the Heidelberg MLA150. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.
These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.
Positive Resist (MLA150)
We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work.
| Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | PEB | Developer | Developer Time | Comments |
|---|---|---|---|---|---|---|---|---|---|---|
| AZ4110 | 4 krpm/30s | 95°C/60s | ~ 1.1 µm | 405 | 240 | 5 | none | AZ400K:DI 1:4 | 50s | Used MLA design (good for isolated lines 0.8-1um) |
| AZ4330 | 4 krpm/30s | 95°C/60s | ~ 3.3 µm | 405 | 320 | 6 | none | AZ400K:DI 1:4 | 90s | Used MLA design |
| AZ4620 | ||||||||||
| SPR 220-3.0 | 2.5 krpm/30s | 115°C/90” | ~ 2.7 µm | 405 | 325 | - 4 | 115°C/90s | AZ300MIF | 60s | Used MLA design |
| SPR 955-CM0.9 | 3 krpm/30s | 95°C/90” | ~ 0.9 µm | 405 | 250 | - 7 | 110°C/90s | AZ300MIF | 60s | Used MLA design |
| THMR-3600HP | 1.5 krpm/45s250 rpm/s | 100°C/60s | 0.430µm | 405 | 180–220 | -4 | 100°C/60s | AZ300MiF | 20s | ~0.4nm line/space:
lower dose for clear-field, higher dose for dark-field. |
Negative Resist (MLA150)
We found that all the negative PR's we tested required the 375nm in order to be fully exposure with reasonable dose.
| Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | PEB | Flood | Developer | Developer Time | Comments |
|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ5214 | 6 krpm/30s | 95°C/60s | ~ 1.0 µm | 375 | 35 | - 5 | 110°C/60s | 60" | AZ300MIF | 60s | Used UCSB design. Good for up to ~1.3um open line space. |
| AZnLOF2020 | 4 krpm/30s | 110°C/60s | ~ 2.1µm | 375 | 340 | - 3 | 110°C/60s | none | AZ300MIF | 90s | Used UCSB design. Good for 2um open line space. |
| SU-8 2075 | ~70µm | 375 | Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. |
Greyscale Lithography (MLA150)
AZ4620 is the manufacturer-recommended PR for greyscale litho.
| Resist | Spin Cond. | Bake | Thickness | Exposure Dose (mJ/cm2) | Focus Offset | PEB | Flood | Developer | Developer Time | Comments |
|---|---|---|---|---|---|---|---|---|---|---|
| AZ4620 | – krpm/30” | 95°C/60” | 60" | AZ300MIF | 60" |
|