S-Cubed Flexi - Operating Procedure: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
initial secitons, draft only
 
inital procedure, and initial recipes
Line 1: Line 1:
{{WIP}}
{{WIP}}
'''Only staff & designated maintenance users are allowed to write recipes on this tool!
'''Only staff & designated maintenance users are allowed to write recipes on this tool! '''
Maintaining low particle counts on this tool is extremely important, so users must strictly follow the training procedures.'''
Maintaining low particle counts on this tool is extremely important, so users must strictly follow the training procedures. The Underside of your wafers must be clean to avoid contamination!
Processes currently available to lab users:


* DS-K101 BARC (can be used like DUV42P)
⚫
== Initial ==
* UV6 Positive DUV Resist
make sure system is not running, is on correct screen etc.
* ''(PMGI and PMMA not yet available for general use)''


⚫
===Initial===
Check liquids


* Make sure system is not running a process - Lot view shows no wafers or batches running.
CHeck if nozzle has been cleaned, TBD?


* Check liquid supplies
RUn a test wafer, look for uniformity.
** Check PR + EBR bottles by weight (lift by hand).  Replace EBR if needed, just unscrew and put into new bottle. If PR bottle empty (see large bubbles in tube) let TonyB/SeanD know, <u>not user replaceable</u>.


(If running PMGI, check if nozzles cleaned)
== Wafer Load ==
TBD, including check


* Check PR nozzle "bath" - make sure it's not clogged (should have a bit of liquid, but not above drain hole).  If it does, use wooden stick of swab to unclog.
⚫
== Run Recipe ==

* Check if hot plates are set to the needs temperatures. If not, run Temp-change recipe:

# Load dummy wafer (clean underside)
# run recipe: Staff>SET-<HP#>-<TEMP> recipe corresponding to needed temp.
## Eg. '''Staff > SET-HP4-220C''' will set hotplate 4 to 220°C
# Check that hotplate reach desired temp.(will overshoot by ~2-3°C)
# After 5min bake, need +/-2°C before running process.

⚫
=== Run Wafers ===

* Load test "mechanical" wafer - run a test run of your desired recipe, make sure spin looks ok.  Important for first UV6 run after >6hrs idle.  1st Mechanical wafer will likely show radial nonuniformity as dried PR is ejected.  2nd test wafer should spin with high uniformity.

* Load your wafers into Left Cassette, run your Route.  Use filter ONLY [Staff].

<br />

=== Allowed Recipes ===
{| class="wikitable"
|+''Ask [[Tony Bosch|Staff]] if you need a new recipe.''
|
|'''<u>Route/Chain</u>'''
|'''<u>Name</u>'''
|'''<u>Spin Speed</u>'''
|'''<u>Bake Temp</u>'''
|'''<u>Notes</u>'''
|-
|'''DS-K101 recipes'''
|Route
|Coat-DS-K101-304[5Krpm]-185C
|
|
|
|-
|'''UV6 Recipes'''
|Route
|Staff > Coat-UV6[3.5K]-135C
|3.5krpm
|135°C
|
|-
|'''DS-K101 + UV6 Recipes'''
|Chain
|Staff > Coat-DSK101[5K]-220C-UV6[3.5K]-135C
|DSK: 5krpm
UV6: 3.5krpm
|DSK: 220°C
UV6: 135°C
|
|-
|'''Hotplate Set recipes'''
|Route
|SET-HP4-220C
|
|
|Check that hotplate 4 (top) is between 218-222°C when done.
|-
|
|
|
|
|
|
|}
'''NEVER RUN DEVELOPER RECIPES on this machine!'''

The developer recipes are prone to damage the hardware if not handled correctly - system is <u>NOT AVAILABLE for automated develop</u> at this time.

Revision as of 23:05, 2 May 2022


Work In Progress

This article is still under construction. It may contain factual errors. Content is subject to change.


Only staff & designated maintenance users are allowed to write recipes on this tool!  
Maintaining low particle counts on this tool is extremely important, so users must strictly follow the training procedures. The Underside of your wafers must be clean to avoid contamination!

Processes currently available to lab users:

  • DS-K101 BARC (can be used like DUV42P)
  • UV6 Positive DUV Resist
  • (PMGI and PMMA not yet available for general use)

Initial

  • Make sure system is not running a process - Lot view shows no wafers or batches running.
  • Check liquid supplies
    • Check PR + EBR bottles by weight (lift by hand).  Replace EBR if needed, just unscrew and put into new bottle. If PR bottle empty (see large bubbles in tube) let TonyB/SeanD know, not user replaceable.

(If running PMGI, check if nozzles cleaned)

  • Check PR nozzle "bath" - make sure it's not clogged (should have a bit of liquid, but not above drain hole).  If it does, use wooden stick of swab to unclog.
  • Check if hot plates are set to the needs temperatures. If not, run Temp-change recipe:
  1. Load dummy wafer (clean underside)
  2. run recipe: Staff>SET-<HP#>-<TEMP> recipe corresponding to needed temp.
    1. Eg. Staff > SET-HP4-220C will set hotplate 4 to 220°C
  3. Check that hotplate reach desired temp.(will overshoot by ~2-3°C)
  4. After 5min bake, need +/-2°C before running process.

Run Wafers

  • Load test "mechanical" wafer - run a test run of your desired recipe, make sure spin looks ok.  Important for first UV6 run after >6hrs idle.  1st Mechanical wafer will likely show radial nonuniformity as dried PR is ejected.  2nd test wafer should spin with high uniformity.
  • Load your wafers into Left Cassette, run your Route.  Use filter ONLY [Staff].


Allowed Recipes

Ask Staff if you need a new recipe.
Route/Chain Name Spin Speed Bake Temp Notes
DS-K101 recipes Route Coat-DS-K101-304[5Krpm]-185C
UV6 Recipes Route Staff > Coat-UV6[3.5K]-135C 3.5krpm 135°C
DS-K101 + UV6 Recipes Chain Staff > Coat-DSK101[5K]-220C-UV6[3.5K]-135C DSK: 5krpm

UV6: 3.5krpm

DSK: 220°C

UV6: 135°C

Hotplate Set recipes Route SET-HP4-220C Check that hotplate 4 (top) is between 218-222°C when done.
NEVER RUN DEVELOPER RECIPES on this machine!
The developer recipes are prone to damage the hardware if not handled correctly - system is NOT AVAILABLE for automated develop at this time.