ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec
Date
Sample#
Etch Rate (nm/min)
Etch Selectivity (SiO2/PR)
Averaged Sidewall Angle (
o
)
SEM Images
10/5/2018
SiO2#01
95.2
0.74
77.9
[1]
1/28/2019
I21902
92.1
0.77
[2]
3/6/2019
I21903
88.5
0.80
79.4
[3]
7/12/2019
I21906
91.9
0.69
78.1
[4]
Navigation menu
Personal tools
Create account
Log in
Namespaces
Page
Discussion
English
Views
Read
View source
View history
More
Search
InvisibleMenu
QuickLinks
Lab Rules
Common Questions/FAQ
Staff List
Equipment Signup
Chemicals + MSDS
Equipment
Full Tool List
Lithography
Vacuum Deposition
Dry Etch
Wet Processing
Thermal Processing
Packaging
Metrology & Test
Recipes and Data
Lithography
Vacuum Deposition
Dry Etching
Wet Etching
Thermal Processing
Packaging Tools
Data + Info
Process Control Data
Tutorials
Calculators/Utilities
NanoFab Info
Research + Pubs
Tech Talks
Tools
What links here
Related changes
Special pages
Printable version
Permanent link
Page information