Atomic Layer Deposition Recipes

From UCSB Nanofab Wiki
Revision as of 17:13, 23 April 2020 by John d (talk | contribs) (→Atomic Layer Deposition (Oxford FlexAL): changed to "ask Tool Supervisor" instead of BillM)
Jump to navigation Jump to search

Back to Vacuum Deposition Recipes.

Atomic Layer Deposition (Oxford FlexAL)

Oxford FlexAL Chamber #1: Metals

Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)

Pt deposition (ALD CHAMBER 1)

  • Recipe name: Ch1_TMCpPt+O3-300C
  • Pt deposition rate ~ 0.5-0.6 A/cyc
  • Conductivity data: (to be added)
  • recipe utilizes the ozone generator which must be first set to the following conditions:
    • O2 flow = 250sccm
    • O3 concentration = 15 wt%
  • 300°C Deposition

Ru deposition (ALD CHAMBER 1)

  • Recipe name: Ch1_Ex03Ru[HPbub]+O2-300C
  • Ru deposition rate ~ 0.6-0.7A/cyc.
  • Conductivity data: (to be added)
  • 300°C, O2 gas reaction

ZnO Deposition (ALD Chamber 1)

Conductive film.

  • Recipe name: Ch1_DEZ+H2O-200C
  • ZnO deposition rate ≈ 1.6 A/cycle
  • resistivity ≈ TBA
  • 200°C Deposition, Water reaction

ZnO:Al deposition (ALD CHAMBER 1)

Al-Doped ZnO for variable resisitivity.

  • Recipe name: Ch1_DEZ/TMA+H2O-200C
    • The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.
  • Al dose fraction = 5% for lowest resistivity
  • ZnO deposition rate ~ 1.7A/cyc
  • resistivity ~ 4200uOhm.cm (390A film)

Oxford FlexAL Chamber #3: Dielectrics

Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)

Al2O3 deposition (ALD CHAMBER 3)

  • Recipe name: Ch3_TMA+H2O-300C
    • Al2O3 deposition rate ~ 1A/cyc
    • 300°C Dep., Water reaction
  • Recipe Name: CH3_TMA+H2O-XYZ?
    • TBD

AlN deposition (ALD CHAMBER 3)

  • Recipe name: Ch3_TMA+100W/20N*-300C
    • AlN deposition rate ~ t.b.d.
    • Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
    • 300°C Dep.

HfO2 deposition (ALD CHAMBER 3)

  • Recipe name: Ch3_TEMAH+H2O-300C
    • HfO2 deposition rate ~ 0.9-1.0A/cyc
    • Note: deposition shows significant parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
    • 300°C Dep.

SiO2 deposition (ALD CHAMBER 3)

  • Recipe name: Ch3_TDMAS+250W/O*-300C
    • SiO2 deposition rate ~ 0.7-0.8A/cyc
    • Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.

ZrO2 deposition (ALD CHAMBER 3)

  • Recipe name: Ch3_TEMAZ+H2O-300C
    • ZrO2 deposition rate ~ 0.9-1.0A/cyc
    • Not directly characterized since results are basically the same as the HfO2 process above.
    • 300°C Dep.

TiO2 deposition (ALD CHAMBER 3)

  • Recipe name: Ch3_TDMAT+H2O-300C
    • TiO2 deposition rate ~ 0.6A/cyc
    • Note: deposition shows parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
    • 300°C Dep.

TiN deposition (ALD CHAMBER 3)

  • Recipe name: Ch3_TDMAT+N*/H*-300C
    • TiN deposition rate ~ 0.7A/cyc
    • Conductivity data: (to be added)
    • 300°C Dep, uses Plasma of N2 & H2 gases.