Data - InP Ridge Etch (Oxford ICP Etcher)



Work In Progress

This article is still under construction. It may contain factual errors. Content is subject to change.


InP Ridge Etch: 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min05sec (305sec)
Date Sample# Etch Rate (nm/min) Etch Selectivity (InP/SiO2) Comments SEM Images
1/11/22 DJ_Cal 0.602 64.6nm left Software timing bugs fixed - new etch rate will appear slightly higher. [1]
1/12/22 DJ_Cal02 0.563 76.4nm left [2]
1/12/22 DJ_Cal03 0.612 80.1nm left [3]