Lift-off DUV Lift-off: LOR Underlayers

From UCSB Nanofab Wiki
Revision as of 22:31, 23 September 2026 by John d (talk | contribs) (alex spott's recipe)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)
Jump to navigation Jump to search

LOR30C

  1. Dehydrate (O2 plasma or 150°C, 2 min+), no adhesion promoter
  2. Spin LOR30C at various speeds depending on thickness desired
    1. See datasheet for spin-curves.
  3. 180°C, 4 min
  4. Spin/bake imaging layer - according to Imaging PR recipe
  5. Expose ASML
  6. Post-bake imaging layer - according to Imaging PR recipe
  7. Develop AZ 300MiF - varies:
    1. Develop times range between 2 min to as long as 6 or 8 minutes (it's consistent for the same mask and same materials, but varies for process steps, topography, and materials).
  8. Strips in 80C NMP 20–30 min

Pros: Thick in a single layer, excellent coverage for tall features, varying topography, and filling vias. Rarely has cracking issues, no ramp baking required, typically minimal bubbles from feature corners.

Cons: High and uncontrollable undercut. You can't switch to flood expose / 101A like you can with PMGI so you're stuck with the undercut you get whenever it's done developing. Not suitable for close features.

Contributed by Alex Spott.