Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point. | Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point. | ||
Line 10: | Line 10: | ||
'''''Any I-Line PR is usable''''', although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR. | '''''Any I-Line PR is usable''''', although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR. | ||
− | === Positive Resist (MLA150) === | + | ===Positive Resist (MLA150)=== |
''We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias [[MLA150 - Design Guidelines#High-Resolution Writing|as described here]].'' | ''We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias [[MLA150 - Design Guidelines#High-Resolution Writing|as described here]].'' | ||
Line 104: | Line 104: | ||
lower dose for clear-field, higher dose for dark-field. | lower dose for clear-field, higher dose for dark-field. | ||
+ | |- | ||
+ | | colspan="11" |*PEB: Post-exposure bake | ||
|} | |} | ||
− | === Negative Resist (MLA150) === | + | ===Negative Resist (MLA150)=== |
''We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.'' | ''We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.'' | ||
Line 162: | Line 164: | ||
| | | | ||
|Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. | |Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. | ||
+ | |- | ||
+ | | colspan="12" |*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal, and requires flood exposure with the MA6 or MJB aligner afterwards, before develop. | ||
|} | |} | ||
− | === Greyscale Lithography (MLA150) === | + | ===Greyscale Lithography (MLA150)=== |
''AZ4620 is the manufacturer-recommended PR for greyscale litho.'' | ''AZ4620 is the manufacturer-recommended PR for greyscale litho.'' | ||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" | {| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
Revision as of 21:58, 30 June 2022
Maskless Aligner (Heidelberg MLA150)
Photolithography Recipes for the Heidelberg MLA150. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.
These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.
Any I-Line PR is usable, although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR.
Positive Resist (MLA150)
We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias as described here.
Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.
Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | PEB | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
AZ4110 | 4 krpm, 30s | 95°C, 60s | ~ 1.1 µm | 405 | 240 | 5 | none | AZ400K:DI 1:4 | 50s | Used HIMT design (good for isolated lines 0.8-1um) |
AZ4330 | 4 krpm, 30s | 95°C, 60s | ~ 3.3 µm | 405 | 320 | 6 | none | AZ400K:DI 1:4 | 90s | Used HIMT design |
AZ4620 | ||||||||||
SPR 220-3.0 | 2.5 krpm, 30s | 115°C, 90s | ~ 2.7 µm | 405 | 325 | - 4 | 115°C, 90s | AZ300MIF | 60s | Used HIMT design. 0.6-0.9µm line/space. |
SPR 955-CM0.9 | 3 krpm, 30s | 95°C, 90s | ~ 0.9 µm | 405 | 250 | - 7 | 110°C, 90s | AZ300MIF | 60s | Used HIMT design |
THMR-3600HP | 1.5 krpm, 45s;
250 rpm/s |
100°C, 60s | 0.430µm | 405 | 180–220 | -4 | 100°C, 60s | AZ300MiF | 20s | ~0.4nm line/space:
lower dose for clear-field, higher dose for dark-field. |
*PEB: Post-exposure bake |
Negative Resist (MLA150)
We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.
Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|---|
AZ5214 | 6 krpm, 30s | 95°C, 60s | ~ 1.0 µm | 375 | 35 | - 5 | 110°C, 60s | 60" | AZ300MIF | 60s | Used UCSB design. Good for up to ~1.3um open line space. |
AZnLOF2020 | 4 krpm, 30s | 110°C, 60s | ~ 2.1µm | 375 | 340 | - 3 | 110°C, 60s | none | AZ300MIF | 90s | Used UCSB design. Good for 2um open line space. |
SU-8 2075 | ~70µm | 375 | Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. | ||||||||
*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal, and requires flood exposure with the MA6 or MJB aligner afterwards, before develop. |
Greyscale Lithography (MLA150)
AZ4620 is the manufacturer-recommended PR for greyscale litho.
Resist | Spin Cond. | Bake | Thickness | Exposure Dose (mJ/cm2) | Focus Offset | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
AZ4620 | ? krpm/30” | 95°C, 60” | 60" | AZ300MIF | 60s |
|