# Mount sample such that area to be monitored is located in the laser monitor's cutout window, as indicated by the Carrier wafer mounted to the tool and/or the glass slide showing the laser monitor location. | # Mount sample such that area to be monitored is located in the laser monitor's cutout window, as indicated by the Carrier wafer mounted to the tool and/or the glass slide showing the laser monitor location. | ||
## The locations on ICP#1 and ICP#2 are different. | ## The locations on ICP#1 and ICP#2 are different. | ||
Line 38: | Line 41: | ||
## '''<u>ICP#1:</u>''' | ## '''<u>ICP#1:</u>''' | ||
### OPTIONALLY: Set switch to "MR" to use side keyboard/screen/manual box (make sure Manual Box has "Evacuate" enabled on all chambers!) | ### OPTIONALLY: Set switch to "MR" to use side keyboard/screen/manual box (make sure Manual Box has "Evacuate" enabled on all chambers!) | ||
− | #### You must set this back to CR when you are done! | + | #### You must set this back to "CR" when you are done! |
### {Test} mode soft-button (should already be enabled) | ### {Test} mode soft-button (should already be enabled) | ||
### F6 Test | ### F6 Test | ||
Line 73: | Line 76: | ||
### {Start} soft button. Will check all three chambers before removing your wafer, takes a while. Do not touch until screen says "STOP" on top-left. | ### {Start} soft button. Will check all three chambers before removing your wafer, takes a while. Do not touch until screen says "STOP" on top-left. | ||
### {Auto} soft-button for normal operation (to run your clean etc.) | ### {Auto} soft-button for normal operation (to run your clean etc.) | ||
− | ### '''Set side back to CR if changed the switch.''' | + | ### '''Set side back to CR if you changed the switch.''' |
## <u>'''ICP#2 Unload:'''</u> | ## <u>'''ICP#2 Unload:'''</u> | ||
### Return to main menu | ### Return to main menu | ||
Line 81: | Line 84: | ||
## End Laser Monitoring / Save Data: | ## End Laser Monitoring / Save Data: | ||
### [Force Cut] | ### [Force Cut] | ||
− | ### Save Data if desired (Right-click the plots, copy data into Notepad etc.) | + | ### Save Data if desired (Right-click the plots, copy data into Notepad, save BMP etc.) |
− | ### Turn off Illumination & Unplug Laser Interlock Key from Laser Head. | + | ### Turn off Camera Illumination & Unplug Laser Interlock Key from Laser Head. |
Revision as of 00:47, 15 May 2019
Procedure for performing an etch with laser monitor endpoint on the Panasonic ICP etchers.
Demis D. John, 2019-05-15
- Mount sample such that area to be monitored is located in the laser monitor's cutout window, as indicated by the Carrier wafer mounted to the tool and/or the glass slide showing the laser monitor location.
- The locations on ICP#1 and ICP#2 are different.
- Load wafer into etch chamber
- ICP#1 Manual Load:
- {Test} Mode soft-button
- Remove all wafers from cassettes
- Place only your sample wafer in the bottom slot (#1) on left cassette (No. 1)
- Check that cassette is seated properly. It will not map the cassette!
- F6 Test
- F1 Wf. Trans.
- F1 Wf TRWIN ("Throw In")
- Confirm that Wafer #1 will be transferred into the E-Ch. ("Etching Chamber")
- {Start} soft-button
- ICP#2 Manual Load:
- {Test} Mode soft-button
- Place Carrier wafer in load slot
- Menu Test > Trans/Test > Transport > Wafer Load
- {Start} soft-button
- ICP#1 Manual Load:
- Edit your ICP Recipe, make sure Step Time is longer than expected to stop using the Manual Box instead.
- Laser Monitor Setup:
- Launch "uEye" Camera software.
- Start Camera feed
- Enable "Auto Contrast"
- Enable "Fit to Window"
- Turn on Illumination on laser head.
- Plug in Laser Interlock to turn on laser (RF connector on keychain)
- Should see laser spot on wafer immediately. Can only see laser spot if a wafer is in the chamber, and laser is projected through the cutouts in the chamber heaters/casing.
- Adjust focus (small changes only), to minimize size of laser spot.
- GREY knobs ONLY to adjust X/Y. Place Laser on region to be monitored.
- Do NOT adjust the Black tilt knobs! If you are not an optics guru, then you usually will only make a mess of this.
- Launch "Etch Director 2" Laser monitoring software
- Check that Signal level is live (non-zero). Can block laser head with hand to ensure signal shows dramatic change.
- Make sure "Endpoint" panel does Not have "Accept" or "Auto Go" checked on any of the Endpoint tabs, or it may stop recording at some point.
- Make sure you have your simulation or a screenshot of the expected stopping point handy.
- {Start} & {Go} to begin laser monitoring
- Launch "uEye" Camera software.
- Run your etch in "Process Test" Mode:
- ICP#1:
- OPTIONALLY: Set switch to "MR" to use side keyboard/screen/manual box (make sure Manual Box has "Evacuate" enabled on all chambers!)
- You must set this back to "CR" when you are done!
- {Test} mode soft-button (should already be enabled)
- F6 Test
- F2 Test
- F1 Etch Test
- F2 Selection
- Choose your recipe, edit if needed
- F4 Register
- {Start} soft-button
- F5 & F5 to exit out to main menu
- F3 Monitor > F1 E-Ch. to monitor the etch
- OPTIONALLY: Set switch to "MR" to use side keyboard/screen/manual box (make sure Manual Box has "Evacuate" enabled on all chambers!)
- ICP#2:
- {Test} mode soft-button (should already be enabled)
- Menu [Test]
- [Process Test]
- [Etch Test]
- ¿ [Selection]
- Choose your recipe, edit if needed
- [Register]
- {Start} soft-button
- Return & Return to exit out to main menu
- Monitor > P/C1 to monitor the etch
- ICP#1:
- Manual Box (Paddle) to End Step at the appropriate time according to laser monitor (eg. some overetch after reaching desired endpoint)
- ICP#1: [RF__ OFF] button to end current step. Make sure you use the correct Manual Box, there is one at each side of the tool (CR and MR sides)!
- ICP#2: [Process Skip] to end current step.
- Wait for decharge steps to complete, done when top-left of screen "RUN" changes to "STOP"
- Transfer wafer out of chamber:
- ICP#1 Unload:
- Return to main menu
- F6 Test
- F1 Wf. Trans.
- F2 Collect
- Double-Check that all cassettes are EMPTY and seated properly
- {Start} soft button. Will check all three chambers before removing your wafer, takes a while. Do not touch until screen says "STOP" on top-left.
- {Auto} soft-button for normal operation (to run your clean etc.)
- Set side back to CR if you changed the switch.
- ICP#2 Unload:
- Return to main menu
- Menu Test > Trans/Test > Transport > Wafer Unload
- {Start} soft-button. Do not touch until screen says "STOP" on top-left.
- {Auto} soft-button for normal operation (to run your clean etc.)
- End Laser Monitoring / Save Data:
- [Force Cut]
- Save Data if desired (Right-click the plots, copy data into Notepad, save BMP etc.)
- Turn off Camera Illumination & Unplug Laser Interlock Key from Laser Head.
- ICP#1 Unload: