+ | |+'''ICP#1 Recipe:''' 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec |
+ | | colspan="5" | |
||
| |
| |
||
|- |
|- |
Revision as of 08:12, 23 April 2020
Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) | SEM Images |
1/28/2019 | I11901 | 110 | 1.35 | see SEM → | [1] |
5/29/2019 | I11903 | 105 | 1.41 | [2] | |
1/13/2020 | I12001 | 78.0 | 1.06 | unusual - two regions | [3] |
Rate on 1/13/2020 is low by ~20%, so chamber was wet-cleaned on 1/21/2020. Data below for 1/23 shows rate returned to "normal". | |||||
1/23/2020 | I12002 | 109 | 1.16 | [4] | |
2/28/2020 | I12003 | 119 | 1.17 | 56.6 | [5] |
Sidewall profile on 2/28/2020 etches is slanted, chamber will be wet-cleaned on 3/2/2020 and re-tested. Data below shows etch returned to "normal". | |||||
3/3/2020 | I12004 | 110 | 1.05 | [6] |