OLD - PECVD2 Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Line 2: Line 2:
== SiN deposition (PECVD #2) ==
== SiN deposition (PECVD #2) ==
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data August 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data September 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]



Revision as of 22:12, 24 September 2014

PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.957
  • Stress ≈ 499MPa
  • HF etch rate:~49nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.50 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.474
  • Stress ≈ -252MPa
  • HF etch rate~616nm/min

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.14 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.935
  • Stress ≈ -7.18MPa
  • HF etch rate~48nm/min

Amorphous-Si deposition (PECVD #2)