OLD - PECVD2 Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
| Line 17: | Line 17: | ||
== SiO<sub>2</sub> deposition (PECVD #2) == |
== SiO<sub>2</sub> deposition (PECVD #2) == |
||
*[[media:Advanced PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe]] |
*[[media:Advanced PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe]] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014] |
||
Revision as of 17:12, 11 December 2014
PECVD 2 (Advanced Vacuum)
Photos
SiN deposition (PECVD #2)
- Deposition Rate: ≈ 7.93 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.961
- Stress ≈ 495MPa
- HF etch rate:~49nm/min
SiO2 deposition (PECVD #2)
- Deposition Rate: ≈ 28.64 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.475
- Stress ≈ -260MPa
- HF etch rate~623nm/min
LS SiN deposition (PECVD #2)
- Deposition Rate: ≈ 7.87 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.938
- Stress ≈ 1.76MPa
- HF etch rate~47nm/min