ASML Stepper 3 Standard Operating Procedure: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Running a focus and/or exposure matrix: discussion of "process window" and "tolerance"
pasted from Word Doc rev. 2022-08-23 DJ
Line 3: Line 3:
==Normal User Procedures==
==Normal User Procedures==


===Cleaning the back-sides of wafers  ===
# Cleaning the back-sides of wafers:  '''<u>Very important</u>'''
## Make sure all work surfaces/spin chucks/hot plates are cleaned!  Don’t use wipes, place baked wafers directly on cleaned steel surfaces.
Very important! '''It is crucial that particles do not get tracked into the system's exposure chuck'''. Sub-micron features will have resolution issues if a particle alters the local wafer focus, affecting everyone's processes.
## Cleaning residue of DUV42P or DSK101 (BARC’s):  This technique is much better than trying to wipe.  Use clean gloves and hold the wafer edges with your hands.  

### After spin coating, BEFORE baking, place wafer upside down in POLOS spinner using non-contact chuck.  
#Make sure all work surfaces/spin chucks/hot plates are cleaned!  Don’t use wipes, instead place baked wafers directly on cleaned steel surfaces.
### Set spin speed to 2000rpm.  Program “backside”.
#Cleaning residue of AR2 or DSK101:  This technique is much better than trying to wipe.  Use clean gloves and hold the wafer edges with your hands.  
### Spin wafer, wait until at top speed.
##After spin coating, place wafer upside down in POLOS spinner using non-contact chuck.  
### Squirt “Remover PG” 10sec, then Acetone 3 seconds, then ISO for 3 sec.
##Set spin speed to 2000rpm.  
### Spin Dry while blowing with N2.  Wait ~5sec before stopping spin.
##Spin wafer, wait until at top speed.
### Remove wafer and do bake as normal.
##Squirt Acetone on sample back for 3 seconds. Followed by ISO for 3 sec.
## Cleaning residues of DUV PR’s such as: UV210, UV6, UVN2300:
##Spin Dry while blowing with N2.
### After baking, place wafer face-down in POLOS spinner using non-contact chuck.
##Remove wafer and do bake as normal
### Set spin speed to 2000rpm.   Program “backside”
#Cleaning residues of UV210, UV6, UNV2300, or PEK-162C1
### Spin wafer, wait until at top speed.
##After baking and cooling, place wafer upside down in POLOS spinner using non-contact chuck.
### Squirt Acetone on sample back for 3 seconds.  Followed by ISO for 3 sec.
##Set spin speed to 2000rpm.
##Spin wafer, wait until at top speed.
### Spin Dry while blowing with N2.
## Bring wafers and ASML cassette to Solvent bench, ensure surfaces are clean from solvents.
##Squirt Acetone on sample back for 3 seconds. Followed by ISO for 3 sec.
## Check back-side of wafer thoroughly for particulates before loading into system!  If you see particulates, try to blow then off with high N2 flow first. You may need to get physical with a razor blade to remove stubborn particles.
##Spin Dry while blowing with N2.
### Do this in the solvent bench where HEPA filters keep the air cleaner.
#Check back-side of wafer thoroughly for particulates before loading into system!  If you see particulates, try to blow then off with high N2 flow first, you may need to get physical with a razor blade to remove stubborn particles.
# Reticle Unloading  and Loading

## (Mat Hdl) Material Handler (button near top right of software window)
===Reticle Unloading  and Loading===
### Remove reticles from machine

### Exchange reticle box
#Material Handler '''(Mat Hdl)''' button near top right of main software window
### Unlock box3
##Remove reticles from machine
## Physically Remove desired reticle pod(s), green “3” indicator at box should be lit and all reticles should be lifted up into pod.
##Exchange reticle box
## Use manual box opener to open reticle box.  Move arm slowly.  
##Unlock Box #3
## Remove Pod Lid
###Only box 3 is for general use.
## Remove (or add) reticle to pod.  
#Physically Remove desired reticle pod(s), green indicator at box should be lit and all reticles should be up inside box, not down into machine.
### Two stars on reticle should be in front
#Use manual box opener to open reticle box.  Move arm slowly.
### Chrome (dark) side down
#Remove Pod Lid
## Place Pod lid back on
#Remove (or add) reticle to pod.  Two stars ('''*''') on reticle should be in front.
## Close Pod using arm, move arm slowly
#Place Pod lid back on
## Place Pod back in stepper
#Close Pod using arm, move arm slowly
## Read desired pods
#Place Pod back in stepper
## Go back to main menu once mask barcodes are all showing on screen
#'''(Read)''' Box #3 - takes a few minutes
# Wafer Load
#Exit the Material Handler. The Material Handler can be run in parallel with other operations.
## Open lid, Remove cassette

## (make sure backs of wafers are extremely clean!  No Particles! No residues!  Be extra careful and attentive to this detail!  See above cleaning procedure)  
===Wafer Load===
## Place wafers in slots

## Place cassette back.  Make sure cassette is pulled back snugly in place
*#Open lid, Remove cassette
## Close Lid.
*#Clean underside of wafers thoroughly, looking very carefully for particles.
# Running a Job – Normal operation
*##'''Make sure backs of wafers are extremely clean!'''  No Particles! No residues!  Be extra careful and attentive to this detail!  See Brian Thibeault for instructions.
## Batch Control > Task Streaming
*#Place wafers in slots
## Wait until wafers are read by machine
*#Place cassette back.  Make sure cassette is pulled ''back &'' snugly in place
## Task: Batch > (Append)
*#Close Lid.
## Enter Batch ID first, Hit Return to apply change

## Press Select Button under Job Name and navigate to your job
===Running a Job – Normal operation===
## Click on Layer ID to get a list of layers you can expose: Select layer you want

## Enter number of wafers in Batch Size
*#Batch Control
## Batch Type is “P” for production run (see below for doing a FEM)
*##Task Streaming
## Verify Energy, Focus Offset, Ilumination Mode, NA, Sigma and change as desired
*###Wait until wafers are read by machine
## Hit Action > (Apply) button to register all changes
*###Ensure all other job's status is "Completed" or "Aborted".
## Press (Accept) Button at Top
*###Task: '''Append Batch''' (or select a previous batch and copy)
## Press Queue > (Continue) Button to execute batch.
*###Enter Batch ID first, Hit Return to apply change
## If Batch has general failure:
*###Press '''Select''' Button under Job Name and navigate to your job
*###Click on '''Layer ID''' to get a list of layers you can expose: Select layer you want to shoot.
### Click the (HELP) button on error window and photograph the error chain - send to supervisor if needed.
### Choose “clear litho cluster” option to remove all wafers to output Port.
*###Enter number of wafers in '''Batch Size'''
*###Batch Type is P for production run (see below for doing a FEM)
*###Verify ''Energy'', ''Focus Offset'', ''Ilumination Mode'', ''NA'', ''Sigma'' and change as desired
*####Click through the Images to be shot by this Layer and verify for each Image.
*####Click through the Images to be shot by this Layer, and make sure all the "Reticle ID" shown are loaded into the Reticle system. (Toggle the "View" button on the System View to see loaded Reticle ID's.)
*###Hit Action: '''Apply''' button to register all changes
*###Press '''Accept''' Button at Top
*###Press '''Continue''' Button to execute batch. (May be a short delay before this becomes active.)
*###If batch has general failure:  
*###On the “Abort Batch” error window: click (HELP) button to see the cause of error - photograph this screen. Then Choose the ('''clear litho cluster''') option
*###unload your Reticle when done, follow procedure above.


===Running a focus and/or exposure matrix===
===Running a focus and/or exposure matrix===
Line 86: Line 76:
#When the batch is complete, select the batch in the Task ist, and click '''Batch:''' '''(Report)'''. The '''"Test Exposure Data"''' section of the report shows the exposure params for each die location. This is very useful during your inspection, and it is recommended that you bring a photograph or copy of this exposure matrix table with you when inspecting on the microscope/SEM.
#When the batch is complete, select the batch in the Task ist, and click '''Batch:''' '''(Report)'''. The '''"Test Exposure Data"''' section of the report shows the exposure params for each die location. This is very useful during your inspection, and it is recommended that you bring a photograph or copy of this exposure matrix table with you when inspecting on the microscope/SEM.


==== Tips for FEM analysis ====
====Tips for FEM analysis====
You need to find the '''center of the ''Viable Process Window''''' - meaning you need to see the BAD dose (too high + too low) and BAD focus (too high + too low) then choose a Dose+Focus in the ''middle'' of this range. This allows your process to work even if the focus or some other process varies.
You need to find the '''center of the ''Viable Process Window''''' - meaning you need to see the BAD dose (too high + too low) and BAD focus (too high + too low) then choose a Dose+Focus in the ''middle'' of this range. This allows your process to work even if the focus or some other process varies.



Revision as of 23:13, 24 August 2022

Regular Procedures for ASML Deep-UV Stepper #3

Normal User Procedures

  1. Cleaning the back-sides of wafers:  Very important
    1. Make sure all work surfaces/spin chucks/hot plates are cleaned!  Don’t use wipes, place baked wafers directly on cleaned steel surfaces.
    2. Cleaning residue of DUV42P or DSK101 (BARC’s):  This technique is much better than trying to wipe.  Use clean gloves and hold the wafer edges with your hands.  
      1. After spin coating, BEFORE baking, place wafer upside down in POLOS spinner using non-contact chuck.  
      2. Set spin speed to 2000rpm.  Program “backside”.
      3. Spin wafer, wait until at top speed.
      4. Squirt “Remover PG” 10sec, then Acetone 3 seconds, then ISO for 3 sec.
      5. Spin Dry while blowing with N2.  Wait ~5sec before stopping spin.
      6. Remove wafer and do bake as normal.
    3. Cleaning residues of DUV PR’s such as: UV210, UV6, UVN2300:
      1. After baking, place wafer face-down in POLOS spinner using non-contact chuck.
      2. Set spin speed to 2000rpm.   Program “backside”
      3. Spin wafer, wait until at top speed.
      4. Squirt Acetone on sample back for 3 seconds.  Followed by ISO for 3 sec.
      5. Spin Dry while blowing with N2.
    4. Bring wafers and ASML cassette to Solvent bench, ensure surfaces are clean from solvents.
    5. Check back-side of wafer thoroughly for particulates before loading into system!  If you see particulates, try to blow then off with high N2 flow first. You may need to get physical with a razor blade to remove stubborn particles.
      1. Do this in the solvent bench where HEPA filters keep the air cleaner.
  2. Reticle Unloading  and Loading
    1. (Mat Hdl) Material Handler (button near top right of software window)
      1. Remove reticles from machine
      2. Exchange reticle box
      3. Unlock box3
    2. Physically Remove desired reticle pod(s), green “3” indicator at box should be lit and all reticles should be lifted up into pod.
    3. Use manual box opener to open reticle box.  Move arm slowly.  
    4. Remove Pod Lid
    5. Remove (or add) reticle to pod.  
      1. Two stars on reticle should be in front
      2. Chrome (dark) side down
    6. Place Pod lid back on
    7. Close Pod using arm, move arm slowly
    8. Place Pod back in stepper
    9. Read desired pods
    10. Go back to main menu once mask barcodes are all showing on screen
  3. Wafer Load
    1. Open lid, Remove cassette
    2. (make sure backs of wafers are extremely clean!  No Particles! No residues!  Be extra careful and attentive to this detail!  See above cleaning procedure)  
    3. Place wafers in slots
    4. Place cassette back.  Make sure cassette is pulled back snugly in place
    5. Close Lid.
  4. Running a Job – Normal operation
    1. Batch Control > Task Streaming
    2. Wait until wafers are read by machine
    3. Task: Batch > (Append)
    4. Enter Batch ID first, Hit Return to apply change
    5. Press Select Button under Job Name and navigate to your job
    6. Click on Layer ID to get a list of layers you can expose: Select layer you want
    7. Enter number of wafers in Batch Size
    8. Batch Type is “P” for production run (see below for doing a FEM)
    9. Verify Energy, Focus Offset, Ilumination Mode, NA, Sigma and change as desired
    10. Hit Action > (Apply) button to register all changes
    11. Press (Accept) Button at Top
    12. Press Queue > (Continue) Button to execute batch.
    13. If Batch has general failure:
      1. Click the (HELP) button on error window and photograph the error chain - send to supervisor if needed.
      2. Choose “clear litho cluster” option to remove all wafers to output Port.

Running a focus and/or exposure matrix

Focus-Exposure Matrix/Arrays (FEM or FEA) are used to determine the proper exposure dose & focus offset for your lithography. Especially important for high-resolution layers. Make sure your entire litho process remains constant (spins, bakes, develop times etc.) between the FEA and your real sample lithos.

  1. Optional: Copy you job to a new job file with the layers/images you want to shoot, but which does not fill the entire wafer to the edges - it instead has only a ~6x6-cm wide array of die (set in the Wafer Layout > Image Distribution section of your program). This ensures that our SEMs can view the full array (The extreme edges of a 4-inch wafer are not possible to image on our SEMs due to motor limits) and simplifies calculations while inspecting the exposed wafer.
  2. Follow "Running a Job" procedure above, until Step 7
  3. Under Batch Type:
    1. Choose E for exposure snake (with flat down, first exposure lower left increments to the right, snakes in serpentine manner around entire wafer).   Enter starting exposure in mJ (bottom-left die) and incremental exposure in mJ (increments up).
    2. Choose F for focus snake (with flat down, first exposure lower left increments to the right, snakes around entire array).   Enter starting focus offset (bottom-left die) and incremental focus for the snake (increments up).
    3. Choose M for Focus-Exposure-Matrix (FEM).  Center cell 0,0 is the nominal Exposure Energy and Focus value you enter.  The array is incremented up and down from the nominal value. By default, exposure Energy varies by columns, Focus by Rows. See schematic below.
  4. Verify non-varied parameters as well as Ilumination Mode, NA, Sigma and change as desired.
  5. Hit Action: (Apply) button to register all changes
    1. Check ALL the Images in the job! Use the (Preset) button to apply to all Images in the job.
  6. Press Accept Button at Top
  7. Press Continue Button to execute batch.
  8. When the batch is complete, select the batch in the Task ist, and click Batch: (Report). The "Test Exposure Data" section of the report shows the exposure params for each die location. This is very useful during your inspection, and it is recommended that you bring a photograph or copy of this exposure matrix table with you when inspecting on the microscope/SEM.

Tips for FEM analysis

You need to find the center of the Viable Process Window - meaning you need to see the BAD dose (too high + too low) and BAD focus (too high + too low) then choose a Dose+Focus in the middle of this range. This allows your process to work even if the focus or some other process varies.

You'll need to decide what "good enough" looks like on your feature inspection - this is your process tolerance. For example instead of looking for "the feature that is exactly 300nm wide", you may want to look for Dose/Focus where "the feature is between 250-350nm, or 300nm±50nm".

A common mistake is to look for "the best die" - but this one good die could be (and often is) at the edge of the working process window, so a small focus variation (wafer thickness or lab temperature) will put your process outside the process window - you'll have chosen a very tight process that easily goes out of spec with random fluctuation in the process.

Stepper 3 - FEM Energy Meander Schematic
Ordering of Energy/Focus for "Meander" mode.
Stepper 3 - FEM Matrix Schematic
Ordering of Exposure Energy/Focus for "Matrix" mode.