Dry Etching Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(updated FL-ICP Si + SIO2 link cuz changed header title)
 
(58 intermediate revisions by 3 users not shown)
Line 1: Line 1:
===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>===
===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>===
<small>''See [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used thin-film depositions.''</small>
<small>''See above [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used dry etches''</small>


===Dry Etching Tools/Materials Table===
===Dry Etching Tools/Materials Table===
''The Key/Legend for this table's <code>A...R6</code> values is at the [[Dry Etching Recipes#Process Ranking Table|bottom of the page]].''

*<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small>
*<small>'''A''': ''Material is available for use, but no recipes are provided.''</small>

{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
|-
! colspan="15" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
| bgcolor="#eaecf0" |<!-- INTENTIONALLY LEFT BLANK -->
! colspan="18" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
! colspan="2" |'''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="4" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
|<!-- INTENTIONALLY LEFT BLANK -->
! colspan="3" |'''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="6" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="5" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
|-
! bgcolor="#d0e7ff" align="center" |'''Material'''
! bgcolor="#d0e7ff" align="center" |'''Material'''
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E646V)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
| bgcolor="#daf1ff" |
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
Line 50: Line 44:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Al
! bgcolor="#d0e7ff" align="center" |Al
|
|
|[[RIE Etching Recipes|R2]]
|
|
|[[RIE Etching Recipes|A]]
|
|
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)|R1}}
|[[ICP Etching Recipes#Al Etch .28Panasonic 2.29|R2]]
|
|
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 2)}}
|
|
|
|
Line 69: Line 60:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Au
! bgcolor="#d0e7ff" align="center" |Au
Line 88: Line 76:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Cr
! bgcolor="#d0e7ff" align="center" |Cr
|
|
|[[RIE Etching Recipes|R2]]
|
|A
|
|
|
|
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
|A
|R1
|
|
|
|
Line 108: Line 92:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Cu
! bgcolor="#d0e7ff" align="center" |Cu
Line 126: Line 108:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ge
! bgcolor="#d0e7ff" align="center" |Ge
Line 136: Line 115:
|
|
|
|
|
|A
|A
|A
|R1
|
|
|
|
Line 144: Line 122:
|
|
|
|
|[[Other Dry Etching Recipes|R2]]
|
|
|
|R1
|A
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Mo
! bgcolor="#d0e7ff" align="center" |Mo
Line 164: Line 140:
|
|
|
|
|
|R1
|
|
|A
|-
|-
!Nb
!Nb
Line 174: Line 147:
|
|
|
|
|
|A
|A
|A
|
|R1
|
|
|
|
|
Line 202: Line 172:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|-
!Os
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
!Os
|
|
|A
|R1
|
|
|
|
|
|
|
|
|A
|A
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Pt
|
|
|
|
Line 225: Line 197:
|
|
|
|
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Pt
|
|
|
|
Line 234: Line 204:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ru
|
|
|
|
|
|
|
|
|A
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R3]]
|
|
|
|
Line 243: Line 218:
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ru
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Si
|
|
|
|
|[[ICP Etching Recipes#DSEIII .28PlasmaTherm.2FDeep Silicon Etcher.29|R6]]
|[[ICP Etching Recipes#Si Etch Recipes (Fluorine ICP Etcher)|R6]]
|
|
|A
|{{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}}
|
|
|R1
|
|
|
|
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ta
|
|
|
|
Line 263: Line 244:
|
|
|A
|A
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Si
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}}
|{{Rl|ICP Etching Recipes|Si Etching}}
|
|
|
|
|A
|
|
|
|
|R1
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ti
|
|
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
|R1
|
|
|A
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Ta
|
|
|
|
Line 289: Line 267:
|
|
|
|
|A
|A
|
|
|R1
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |W
|
|
|
|
|
|
|R2
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
|R1
|
|
|
|
Line 300: Line 282:
|
|
|
|
|A
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ti
|
|
|
|
|R1
|-
!TiW
|
|
|
|
|
|
|R2
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
|A
|
|
|R1
|
|
|
|
Line 319: Line 301:
|
|
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
|
|
|
|
|
Line 328: Line 308:
|
|
|A
|A
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]]
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|
|
|
|
Line 336: Line 316:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
|
|
|
|
|
Line 347: Line 324:
|
|
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
|A
|R1
|
|
|
|
Line 355: Line 332:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |AlGaAs
! bgcolor="#d0e7ff" align="center" |AlGaAs
|
|
|[[RIE Etching Recipes|R3]]
|
|
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}}
|
|
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]]
|
|
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]]
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}}
|
|
|
|
Line 374: Line 348:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |AlGaN
! bgcolor="#d0e7ff" align="center" |AlGaN
Line 385: Line 357:
|
|
|
|
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R2]]
|
|
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R]]
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
Line 393: Line 364:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |AlN
! bgcolor="#d0e7ff" align="center" |AlN
Line 406: Line 375:
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
Line 412: Line 380:
|
|
|
|
|
|R1
|
|A
|-
|-
!BCB
!BCB
|
|
|
|
|
Line 423: Line 388:
|
|
|A
|A
|
|
|
|
|
|
Line 436: Line 399:
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |CdZnTe
! bgcolor="#d0e7ff" align="center" |CdZnTe
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
|[[RIE Etching Recipes|R3]]
|
|
|
|
Line 449: Line 412:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |GaAs
! bgcolor="#d0e7ff" align="center" |GaAs
|
|
|[[RIE Etching Recipes|R4]]
|
|
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}}
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]]
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R2]]
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}}
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}}
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]]
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}}
|
|
|
|
Line 469: Line 428:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |GaN
! bgcolor="#d0e7ff" align="center" |GaN
|
|
|[[RIE Etching Recipes|R4]]
|
|{{rl|RIE Etching Recipes|GaN Etching (RIE 5)}}
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|A
|R1
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R]]
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R6]]
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
Line 489: Line 444:
|
|
|
|
|
|R1
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |GaSb
! bgcolor="#d0e7ff" align="center" |GaSb
|
|
|
|
|
Line 499: Line 452:
|
|
|A
|A
|A
|R1
|A
|R1
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
|
|
|
|
Line 508: Line 460:
|
|
|
|
|
|R1
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
Line 525: Line 476:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |InGaAlAs
! bgcolor="#d0e7ff" align="center" |InGaAlAs
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|[[RIE Etching Recipes|R4]]
|
|
|
|
Line 537: Line 485:
|
|
|
|
|R1
|
|
|A
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
Line 545: Line 492:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |InGaAsP
! bgcolor="#d0e7ff" align="center" |InGaAsP
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|[[RIE Etching Recipes|R4]]
|
|
|
|
Line 556: Line 501:
|
|
|
|
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R3]]
|
|
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]]
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
Line 564: Line 508:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |InP
! bgcolor="#d0e7ff" align="center" |InP
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|[[RIE Etching Recipes|R4]]
|
|
|
|
|
|
|
|A
|A
|A
|R1
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]]
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R6]]
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
Line 585: Line 524:
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|[[Other Dry Etching Recipes|R4]]
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |ITO
! bgcolor="#d0e7ff" align="center" |ITO
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
|[[RIE Etching Recipes|R4]]
|
|
|
|
Line 601: Line 540:
|
|
|
|
|
|R1
|
|
|A
|-
|-
!LiNbO3
!LiNbO3
Line 620: Line 556:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
!Photoresist
!Photoresist & Organics
& ARC
|
|
|[[RIE Etching Recipes|R3]]
|A
|[https://wiki.nanotech.ucsb.edu/wiki/RIE_Etching_Recipes#Photoresist_and_ARC_.28RIE_5.29 R]
|
|
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_.26_ARC_.28Fluorine_ICP_Etcher.29 R]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R]
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]]
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_etching_.28Panasonic_2.29 R]
|
|
|R3
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
|
|
|R
|
|
|R
|
|
|
|R1
|
|
|A
|-
|-
!ARC (Anti Reflective Coating)
!Ru
|
|
|
|
|
|
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]]
|
|
|A
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R]]
|
|
|
|
Line 665: Line 591:
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |SiC
! bgcolor="#d0e7ff" align="center" |SiC
|
|
|
|
|
Line 671: Line 596:
|
|
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
|A
|R1
|
|
|
|
Line 679: Line 604:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |SiN
! bgcolor="#d0e7ff" align="center" |SiN
|
|
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
|
|
|
|
|[[ICP Etching Recipes#Si3N4 Etching .28Fluorine ICP Etcher.29|R3]]
|A
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}}
|[[ICP Etching Recipes#SiNx Etching .28Panasonic 2.29|R3]]
|
|
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]]
|
|
|A
|
|
|
|
|
|
|
|
|
|R1
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
|
|
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
|
|
|
|
|{{rl|ICP Etching Recipes|SiO2 Etching (Fluorine ICP Etcher)}}
|[[ICP Etching Recipes#SiO2 Etch Recipes (Fluorine ICP Etcher)|R6]]
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]]
|
|
|
|
Line 716: Line 635:
|
|
|
|
|[[Other Dry Etching Recipes|R4]]
|
|
|R1
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |SiOxNy
! bgcolor="#d0e7ff" align="center" |SiOxNy
|
|
|
|
|
Line 728: Line 644:
|
|
|A
|A
|A
|R1
|
|
|
|
Line 736: Line 652:
|
|
|
|
|
|R1
|
|A
|-
|-
!SU8
!SU8
|
|
|
|
|
Line 747: Line 660:
|
|
|A
|A
|
|
|
|
|
|
Line 760: Line 671:
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
|
|
|
|
|
Line 766: Line 676:
|
|
|A
|A
|R1
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A]
|
|
|
|
Line 774: Line 684:
|
|
|
|
|
|R1
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |TiN
! bgcolor="#d0e7ff" align="center" |TiN
Line 792: Line 700:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
Line 811: Line 716:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |W-TiW
|
|
|
|
|
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
|A
|
|
|
|
|
|
|
|
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub>
Line 849: Line 732:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |ZnS
! bgcolor="#d0e7ff" align="center" |ZnS
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|[[RIE Etching Recipes|R3]]
|
|
|
|
Line 868: Line 748:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |ZnSe
! bgcolor="#d0e7ff" align="center" |ZnSe
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|[[RIE Etching Recipes|R2]]
|
|
|
|
Line 887: Line 764:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
Line 906: Line 780:
|
|
|
|
|
|R1
|
|
|A
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |'''Material'''
! bgcolor="#d0e7ff" align="center" |'''Material'''
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 1 .28Panasonic E646V.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#ICP Etch 2 .28Panasonic E626I.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
|
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
Line 931: Line 799:
|}
|}


==='''Process Ranking Table'''===
Processes in the table above are ranked by their "''Process Maturity Level''" as follows:
{| class="wikitable"
!Process Level
! colspan="11" |Description of Process Level Ranking
|-
|A
| colspan="11" |Process '''A'''llowed and materials available but never done
|-
|R1
| colspan="11" |Process has been run at least once
|-
|R2
| colspan="11" |Process has been run and/or procedure is documented or/and data available
|-
|R3
| colspan="11" |Process has been run, procedure is documented, and data is available
|-
|R4
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''or''' lookahead/in-situ control available
|-
|R5
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' lookahead/in-situ control available
|-
|R6
| colspan="11" |Process has a documented procedure, regular ( ≥4x per year) data, and control charts & limits available
|}
[[Category:Processing]]
[[Category:Processing]]

Latest revision as of 18:55, 9 March 2025

Process Control Data

See above linked page for process control data (dep rate/stress etc. over time), for a selection of often-used dry etches

Dry Etching Tools/Materials Table

The Key/Legend for this table's A...R6 values is at the bottom of the page.

Dry Etching Recipes
RIE Etching ICP Etching Oxygen Plasma Systems Other Dry Etchers
Material RIE 2
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E646V)
ICP Etch 2
(Panasonic E626I)
Oxford ICP (PlasmaPro 100) Ashers
(Technics PEII)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)
Ag R1
Al R2 R1 R2 R1
Au R4
Cr R2 R1 R1 R1
Cu R1
Ge A R1 R2 R1
Mo R1
Nb A R1
Ni R4
Os A R1
Pt R4
Ru A R3 R1
Si R6 R6 R1 R4 R1
Ta A R1 R1
Ti R1 R1 R1
W R2 R1 R1 R1
TiW R2 R1
Al2O3 A R3 R1
Al2O3 (Sapphire) R1 R1 R1
AlGaAs R3 R1 R3 R1
AlGaN R2 R1
AlN R1
BCB A
CdZnTe R3 R1
GaAs R4 R1 R6 R2 R1
GaN R4 R1 R1 R6 R1
GaSb A R1 R1 R1
HfO2 R1
InGaAlAs R4 R1 R1
InGaAsP R4 R3 R1
InP R4 A R1 R6 R4
ITO R4 R1
LiNbO3 R1
Photoresist & Organics R3 R3 R R3 R3 R3 R3 R1
ARC (Anti Reflective Coating) R3
SiC R1 R1 R1
SiN R3 R1 R3 R3 R1
SiO2 R6 R1 R6 R4 R1
SiOxNy A R1 R1
SU8 A
Ta2O5 A R1 R1
TiN R1
TiO2 R1
ZnO2 R1
ZnS R3 R1
ZnSe R2 R1
ZrO2 R1
Material RIE 2
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
Oxford ICP (PlasmaPro 100) Ashers
(Technics PEII)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)

Process Ranking Table

Processes in the table above are ranked by their "Process Maturity Level" as follows:

Process Level Description of Process Level Ranking
A Process Allowed and materials available but never done
R1 Process has been run at least once
R2 Process has been run and/or procedure is documented or/and data available
R3 Process has been run, procedure is documented, and data is available
R4 Process has a documented procedure with regular (≥4x per year) data or lookahead/in-situ control available
R5 Process has a documented procedure with regular (≥4x per year) data and lookahead/in-situ control available
R6 Process has a documented procedure, regular ( ≥4x per year) data, and control charts & limits available