===<u> |
===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>=== |
||
<small>''See above [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used dry etches''</small> |
<small>''See above [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used dry etches''</small> |
||
| Line 44: | Line 44: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Al |
! bgcolor="#d0e7ff" align="center" |Al |
||
| Line 51: | Line 51: | ||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)|R1}} |
||
| ⚫ | |||
|[https://wiki.nanofab.ucsb.edu/wiki/ICP_Etching_Recipes#Al_Etch_.28Panasonic_2.29 R2] |
|||
| |
| |
||
| |
| |
||
| Line 60: | Line 60: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Au |
! bgcolor="#d0e7ff" align="center" |Au |
||
| Line 76: | Line 76: | ||
| |
| |
||
| |
| |
||
| |
|[[Other Dry Etching Recipes|R4]] |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Cr |
! bgcolor="#d0e7ff" align="center" |Cr |
||
| Line 92: | Line 92: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Cu |
! bgcolor="#d0e7ff" align="center" |Cu |
||
| Line 108: | Line 108: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Ge |
! bgcolor="#d0e7ff" align="center" |Ge |
||
| Line 122: | Line 122: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes|R2]] |
|||
| ⚫ | |||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Mo |
! bgcolor="#d0e7ff" align="center" |Mo |
||
| Line 140: | Line 140: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- |
|- |
||
!Nb |
!Nb |
||
| Line 172: | Line 172: | ||
| |
| |
||
| |
| |
||
| |
|[[Other Dry Etching Recipes|R4]] |
||
|- |
|- |
||
!Os |
!Os |
||
| Line 204: | Line 204: | ||
| |
| |
||
| |
| |
||
| |
|[[Other Dry Etching Recipes|R4]] |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Ru |
! bgcolor="#d0e7ff" align="center" |Ru |
||
| Line 212: | Line 212: | ||
| |
| |
||
|A |
|A |
||
|[ |
|[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R3]] |
||
| |
| |
||
| |
| |
||
| Line 220: | Line 220: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Si |
! bgcolor="#d0e7ff" align="center" |Si |
||
| |
| |
||
| |
| |
||
|[[ |
|[[ICP Etching Recipes#DSEIII .28PlasmaTherm.2FDeep Silicon Etcher.29|R6]] |
||
|[[ICP Etching Recipes#Si |
|[[ICP Etching Recipes#Si Etch Recipes (Fluorine ICP Etcher)|R6]] |
||
| |
| |
||
| |
| |
||
| Line 234: | Line 234: | ||
| |
| |
||
| |
| |
||
| |
|[[Other Dry Etching Recipes|R4]] |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Ta |
! bgcolor="#d0e7ff" align="center" |Ta |
||
| Line 252: | Line 252: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Ti |
! bgcolor="#d0e7ff" align="center" |Ti |
||
| Line 268: | Line 268: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}} |
|||
|R1 |
|||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
|R1 |
|||
| ⚫ | |||
!TiW |
|||
| ⚫ | |||
| ⚫ | |||
| |
|||
|R2 |
|||
| |
|||
|R1 |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
||
| Line 276: | Line 308: | ||
| |
| |
||
|A |
|A |
||
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
|||
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R3] |
|||
| |
| |
||
| |
| |
||
| Line 284: | Line 316: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub> |
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub> |
||
| Line 300: | Line 332: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |AlGaAs |
! bgcolor="#d0e7ff" align="center" |AlGaAs |
||
| Line 316: | Line 348: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |AlGaN |
! bgcolor="#d0e7ff" align="center" |AlGaN |
||
| Line 332: | Line 364: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |AlN |
! bgcolor="#d0e7ff" align="center" |AlN |
||
| Line 348: | Line 380: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- |
|- |
||
!BCB |
!BCB |
||
| Line 380: | Line 412: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |GaAs |
! bgcolor="#d0e7ff" align="center" |GaAs |
||
| Line 388: | Line 420: | ||
| |
| |
||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
||
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]] |
|||
|[https://wiki.nanofab.ucsb.edu/wiki/ICP_Etching_Recipes#GaAs_Etch_.28Panasonic_2.29 R3] |
|||
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29| |
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R2]] |
||
| |
| |
||
| |
| |
||
| Line 396: | Line 428: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |GaN |
! bgcolor="#d0e7ff" align="center" |GaN |
||
| Line 405: | Line 437: | ||
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
||
|R1 |
|R1 |
||
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29| |
|[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R6]] |
||
| |
| |
||
| |
| |
||
| Line 412: | Line 444: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |GaSb |
! bgcolor="#d0e7ff" align="center" |GaSb |
||
| Line 428: | Line 460: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub> |
||
| Line 444: | Line 476: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
||
| Line 460: | Line 492: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |InGaAsP |
! bgcolor="#d0e7ff" align="center" |InGaAsP |
||
| Line 476: | Line 508: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |InP |
! bgcolor="#d0e7ff" align="center" |InP |
||
| Line 492: | Line 524: | ||
| |
| |
||
| |
| |
||
| |
|[[Other Dry Etching Recipes|R4]] |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |ITO |
! bgcolor="#d0e7ff" align="center" |ITO |
||
| Line 508: | Line 540: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- |
|- |
||
!LiNbO3 |
!LiNbO3 |
||
| Line 524: | Line 556: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
!Photoresist |
!Photoresist & Organics |
||
& ARC |
|||
| |
| |
||
|[[RIE Etching Recipes|R3]] |
|[[RIE Etching Recipes|R3]] |
||
| Line 533: | Line 564: | ||
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
||
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R] |
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R] |
||
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
|||
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_etching_.28Panasonic_2.29 R3] |
|||
| |
| |
||
|R3 |
|R3 |
||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
||
| |
| |
||
| |
| |
||
| |
| |
||
|R1 |
|||
|- |
|||
!ARC (Anti Reflective Coating) |
|||
| |
|||
| |
|||
| |
|||
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |SiC |
! bgcolor="#d0e7ff" align="center" |SiC |
||
| Line 557: | Line 604: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |SiN |
! bgcolor="#d0e7ff" align="center" |SiN |
||
| Line 565: | Line 612: | ||
|[[ICP Etching Recipes#Si3N4 Etching .28Fluorine ICP Etcher.29|R3]] |
|[[ICP Etching Recipes#Si3N4 Etching .28Fluorine ICP Etcher.29|R3]] |
||
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
||
|[[ICP Etching Recipes#SiNx Etching .28Panasonic 2.29|R3]] |
|||
|[https://wiki.nanofab.ucsb.edu/wiki/ICP_Etching_Recipes#SiNx_Etching_.28Panasonic_2.29 R3] |
|||
| |
| |
||
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
|[[Oxygen Plasma System Recipes#O2 Ashing|R3]] |
||
| Line 573: | Line 620: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
||
| Line 579: | Line 626: | ||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#SiO2 |
|[[ICP Etching Recipes#SiO2 Etch Recipes (Fluorine ICP Etcher)|R6]] |
||
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
||
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]] |
|||
|[https://wiki.nanofab.ucsb.edu/wiki/ICP_Etching_Recipes#SiO2_Etching_.28Panasonic_2.29 R6] |
|||
| |
| |
||
| |
| |
||
| Line 588: | Line 635: | ||
| |
| |
||
| |
| |
||
| |
|[[Other Dry Etching Recipes|R4]] |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |SiOxNy |
! bgcolor="#d0e7ff" align="center" |SiOxNy |
||
| Line 605: | Line 652: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- |
|- |
||
!SU8 |
!SU8 |
||
| Line 629: | Line 676: | ||
| |
| |
||
|A |
|A |
||
|R1 |
|||
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 R1] |
|||
| |
| |
||
| |
| |
||
| Line 637: | Line 684: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |TiN |
! bgcolor="#d0e7ff" align="center" |TiN |
||
| Line 653: | Line 700: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
||
| Line 669: | Line 716: | ||
| |
| |
||
| |
| |
||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
|R1 |
|R1 |
||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
| ⚫ | |||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub> |
||
| Line 701: | Line 732: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |ZnS |
! bgcolor="#d0e7ff" align="center" |ZnS |
||
| Line 717: | Line 748: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |ZnSe |
! bgcolor="#d0e7ff" align="center" |ZnSe |
||
| Line 733: | Line 764: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
||
| Line 749: | Line 780: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |'''Material''' |
! bgcolor="#d0e7ff" align="center" |'''Material''' |
||
Revision as of 18:55, 9 March 2025
Process Control Data
See above linked page for process control data (dep rate/stress etc. over time), for a selection of often-used dry etches
Dry Etching Tools/Materials Table
The Key/Legend for this table's A...R6 values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been run at least once | ||||||||||
| R2 | Process has been run and/or procedure is documented or/and data available | ||||||||||
| R3 | Process has been run, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data or lookahead/in-situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and lookahead/in-situ control available | ||||||||||
| R6 | Process has a documented procedure, regular ( ≥4x per year) data, and control charts & limits available | ||||||||||