=[[Thermal Evaporator 1]]=
=[[Thermal Evaporator 1]]=


=Materials Table=
==Materials Table==


{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
Line 98: Line 98:
|
|
|
|
|-
|Magnezium
|Mg
|1.74
|5.48
|98.4
|
|
|
|-
|Manganese
|Mn
|7.20
|23.40
|120
|100
|
|
|-
|Nickel
|Ni
|8.90
|26.68
|100
|50
|4.5
⚫
|Used often
|-
|Nichrome
|NiCr
|8.32
|27.59
|
|100
|0.4
|
|-
|Palladium
|Pd
|12.40
|24.73
|140.5
|62
|1.5
|Used often
|-
|Silicon Monoxide
|SiO
|2.13
|10.19
|120
|70
|
|
|-
|Silver
|Ag
|10.5
|16.69
|
|
|
|
|-
|Zinc
|Zn
|7.14
|17.18
|
|50
|4.5
|Used often
|-
|Zinc Oxide
|Zinc Oxide
|ZnO
|ZnO
Line 107: Line 180:
|
|
|-
|-
|Strontium Fluoride
|StrontiumFluoride
|SrF<sub>2
|SrF<sub>2
|4.28
|4.28
Line 126: Line 199:
|-
|-
|ITO(IndiumTinOxide)
|ITO(IndiumTinOxide)
|In<sub>2O<sub>3-SnO<sub>2
|In<sub>2</sub>O<sub>3</sub> - SnO<sub>2
|5.43-7.14
|6.43-7.14
|0.841
|0.841
|
|
Line 135: Line 208:
|-
|-
|Permalloy
|Permalloy
|Ni<sub>0.1Fe<sub>0.2
|Ni<sub>0.1</sub>Fe<sub>0.2</sub>
|8.7
|8.7
|26.40
|26.40
Line 142: Line 215:
|0.1
|0.1
|
|
|-
|}


=[[Thermal Evaporator 2]]=
=[[Thermal Evaporator 2]]=


= Materials Table =
== Materials Table ==


{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
Line 283: Line 356:
|0.841
|0.841
|120
|120
|Used often
|Used often, tooling factor needs adjustment
|-
|-
|Indium antimonide
|Indium antimonide
Line 499: Line 572:
|7.30
|7.30
|0.724
|0.724
|
|197
|Program #9, Tooling factor=200%, cold fixture
⚫
|Used often
|-
|-
|Titanium
|Titanium
Line 571: Line 644:
|
|
|
|
|-
|}

== In Deposition (Thermal Evaporator 2) ==
*[[Media:Thermal evaporator 2-new Sheet1.pdf|Indium evaporation Data]]

Latest revision as of 21:27, 19 June 2025

Back to Vacuum Deposition Recipes.

Thermal Evaporator 1

Materials Table

Thermal Evaporator 2

Materials Table

In Deposition (Thermal Evaporator 2)