Dry Etching Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
Added R6 for GaAs etch on ICP2 |
linked W etch FICP |
||
| (18 intermediate revisions by 2 users not shown) | |||
| Line 3: | Line 3: | ||
===Dry Etching Tools/Materials Table=== |
===Dry Etching Tools/Materials Table=== |
||
==== Process Maturity Ranking ==== |
|||
* <code>'''R6'''</code> - most mature process with regular calibrations recorded on SPC charts. |
|||
* … |
|||
* <code>'''R1'''</code> - least mature - only run once ever. |
|||
''The Key/Legend for this table's <code>A...R6</code> values is at the [[Dry Etching Recipes#Process Ranking Table|bottom of the page]].'' |
''The Key/Legend for this table's <code>A...R6</code> values is at the [[Dry Etching Recipes#Process Ranking Table|bottom of the page]].'' |
||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
||
| Line 76: | Line 83: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes| |
|[[Other Dry Etching Recipes|R3]] |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Cr |
! bgcolor="#d0e7ff" align="center" |Cr |
||
| Line 84: | Line 91: | ||
| |
| |
||
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}} |
||
|[[ICP Etching Recipes#Cr Etching (Panasonic 2)|R3]] |
|||
| ⚫ | |||
| |
| |
||
| |
| |
||
| Line 172: | Line 179: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes| |
|[[Other Dry Etching Recipes|R3]] |
||
|- |
|- |
||
!Os |
!Os |
||
| Line 204: | Line 211: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes| |
|[[Other Dry Etching Recipes|R3]] |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Ru |
! bgcolor="#d0e7ff" align="center" |Ru |
||
| Line 225: | Line 232: | ||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#DSEIII |
|[[ICP Etching Recipes#High Rate Bosch Etch (DSEIII)|R6]], [[ICP Etching Recipes#Silicon: Single-Step, Low Etch Rate, Smooth Sidewall Process (DSEIII)|R3]] |
||
|[[ICP Etching Recipes#Si |
|[[ICP Etching Recipes#Si Etch Recipes (Fluorine ICP Etcher)|R6]] |
||
| |
| |
||
| |
| |
||
| Line 234: | Line 241: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes| |
|[[Other Dry Etching Recipes|R3]] |
||
| |
| |
||
|R1 |
|R1 |
||
| Line 274: | Line 281: | ||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#W Etching (Fluorine ICP Etcher)|R3]] |
|||
| ⚫ | |||
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}} |
||
|R1 |
|R1 |
||
| Line 290: | Line 297: | ||
| |
| |
||
| |
| |
||
| |
|R3 |
||
| |
| |
||
|R1 |
|R1 |
||
| Line 416: | Line 423: | ||
! bgcolor="#d0e7ff" align="center" |GaAs |
! bgcolor="#d0e7ff" align="center" |GaAs |
||
| |
| |
||
|[[RIE Etching Recipes| |
|[[RIE Etching Recipes|R3]] |
||
| |
| |
||
| |
| |
||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|GaAs-AlGaAs Etch (Panasonic 1)}} |
||
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]] |
|[[ICP Etching Recipes#GaAs Etch .28Panasonic 2.29|R6]] |
||
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29| |
|[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R3]] |
||
| |
| |
||
| |
| |
||
| Line 432: | Line 439: | ||
! bgcolor="#d0e7ff" align="center" |GaN |
! bgcolor="#d0e7ff" align="center" |GaN |
||
| |
| |
||
|[[RIE Etching Recipes| |
|[[RIE Etching Recipes|R3]] |
||
| |
| |
||
| |
| |
||
| Line 477: | Line 484: | ||
| |
| |
||
|R1 |
|R1 |
||
| ⚫ | |||
!Hf |
|||
| ⚫ | |||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| ⚫ | |||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
| |
|||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
||
|[[RIE Etching Recipes| |
|[[RIE Etching Recipes|R3]] |
||
| |
| |
||
| |
| |
||
| Line 495: | Line 518: | ||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |InGaAsP |
! bgcolor="#d0e7ff" align="center" |InGaAsP |
||
|[[RIE Etching Recipes| |
|[[RIE Etching Recipes|R3]] |
||
| |
| |
||
| |
| |
||
| Line 511: | Line 534: | ||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |InP |
! bgcolor="#d0e7ff" align="center" |InP |
||
|[[RIE Etching Recipes| |
|[[RIE Etching Recipes|R3]] |
||
| |
| |
||
| |
| |
||
| Line 524: | Line 547: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes| |
|[[Other Dry Etching Recipes|R3]] |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |ITO |
! bgcolor="#d0e7ff" align="center" |ITO |
||
|[[RIE Etching Recipes| |
|[[RIE Etching Recipes|R3]] |
||
| ⚫ | |||
| |
| |
||
| |
| |
||
| Line 534: | Line 556: | ||
| |
| |
||
| |
| |
||
| ⚫ | |||
| |
| |
||
| |
| |
||
| Line 546: | Line 569: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
| |
||
| |
| |
||
| Line 560: | Line 583: | ||
!Photoresist & Organics |
!Photoresist & Organics |
||
| |
| |
||
|[[RIE Etching Recipes|R3]] |
|[[RIE Etching Recipes#Photoresist and ARC (RIE 5)|R3]] |
||
| |
| |
||
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
|[[ICP Etching Recipes#Photoresist .26 ARC .28Fluorine ICP Etcher.29|R3]] |
||
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 |
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R3] |
||
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
|[[ICP Etching Recipes#Al2O3 Etching .28Panasonic 2.29|R3]] |
||
| |
| |
||
| Line 625: | Line 648: | ||
| |
| |
||
| |
| |
||
|[[ICP Etching Recipes#SiO2 Etch (DSEiii)|R3]] |
|||
| ⚫ | |||
|[[ICP Etching Recipes#SiO2 |
|[[ICP Etching Recipes#SiO2 Etch Recipes (Fluorine ICP Etcher)|R6]] |
||
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
||
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]] |
|[[ICP Etching Recipes#SiO2 Etching .28Panasonic 2.29|R6]] |
||
| Line 635: | Line 658: | ||
| |
| |
||
| |
| |
||
|[[Other Dry Etching Recipes| |
|[[Other Dry Etching Recipes|R3]] |
||
|R1 |
|R1 |
||
|- bgcolor="#ffffff" |
|- bgcolor="#ffffff" |
||
| Line 772: | Line 795: | ||
| |
| |
||
| |
| |
||
| |
|R1 |
||
| |
| |
||
| |
| |
||
| Line 799: | Line 822: | ||
|} |
|} |
||
=== |
===Process Ranking Table=== |
||
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
||
{| class="wikitable" |
{| class="wikitable" |
||
| Line 809: | Line 832: | ||
|- |
|- |
||
|R1 |
|R1 |
||
| colspan="11" |Process has been |
| colspan="11" |Process has been ran at least once |
||
|- |
|- |
||
|R2 |
|R2 |
||
| colspan="11" |Process has been |
| colspan="11" |Process has been ran and procedure is documented |
||
|- |
|- |
||
|R3 |
|R3 |
||
| colspan="11" |Process has been |
| colspan="11" |Process has been ran, procedure is documented, and data is available |
||
|- |
|- |
||
|R4 |
|R4 |
||
| colspan="11" |Process has a documented procedure with regular |
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available |
||
|- |
|- |
||
|R5 |
|R5 |
||
| colspan="11" |Process has a documented procedure with regular |
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' in-Situ control available |
||
|- |
|- |
||
|R6 |
|R6 |
||
| colspan="11" |Process has a documented procedure |
| colspan="11" |Process has a documented procedure and control charts/limits available. Controlled process. |
||
|} |
|} |
||
[[Category:Processing]] |
[[Category:Processing]] |
||
Latest revision as of 22:16, 23 September 2026
Process Control Data
See above linked page for process control data (dep rate/stress etc. over time), for a selection of often-used dry etches
Dry Etching Tools/Materials Table
Process Maturity Ranking
R6- most mature process with regular calibrations recorded on SPC charts.- …
R1- least mature - only run once ever.
The Key/Legend for this table's A...R6 values is at the bottom of the page.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been ran at least once | ||||||||||
| R2 | Process has been ran and procedure is documented | ||||||||||
| R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data no in-Situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and in-Situ control available | ||||||||||
| R6 | Process has a documented procedure and control charts/limits available. Controlled process. | ||||||||||