== SiO<sub>2</sub> deposition (PECVD #2) ==
== SiO<sub>2</sub> deposition (PECVD #2) ==
*[[media:Advanced PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe]]
*[[media:Advanced PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe]]
*[[media:ADV OXIDE data April 2014.pdf|Oxide Data (Deposition Rate, Refractive Index, Stress, HF etch rate )]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data April 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data April 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]

Revision as of 01:42, 22 May 2014

PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.29 nm/min
  • Refractive Index: ≈ 1.955
  • Stress ≈ 498MPa
  • HF etch rate:~48nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.36 nm/min
  • Refractive Index: ≈ 1.473
  • Stress ≈ -256MPa
  • HF etch rate~582nm/min

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.34 nm/min
  • Refractive Index: ≈ 1.932
  • Stress ≈ -46MPa

Amorphous-Si deposition (PECVD #2)