=== '''1. Unaxis deposition - 300nm of  SiO2 LDR film @250°C''' ===
=== '''Unaxis deposition - 300nm SiO2 LDR film @250°C''' ===
a) Prepare three 4” wafers:
a) Prepare three 4” wafers:
⚫
* for seasoning (regular Si wafer ~500nm thick)

·     for seasoning (regular Si wafer ~500nm thick)
* for deposition (your wafer for deposition)
⚫
* for cleaning ( Si thick wafer~0.8-1um)

⚫
·     for deposition (your wafer for deposition)

⚫
·     for cleaning ( Si thick wafer~0.8-1um)

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.


c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in the recipe.
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in recipes.
⚫
* Seasoning recipe name: '''SiO2 seasoning''', '''t=2min'''

Seasoning recipe name: '''SiO2 seasoning''', '''t=2min'''
* Deposition recipe name: '''SiO2 LDR 250°C, t=780 sec'''
⚫
* Cleaning recipe name: '''Post dep PD''', '''t=900sec'''

⚫
There is '''only one SiO2 seasoning''' recipe. This same recipe is used for seasoning for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.
Deposition recipe name: S'''iO2 LDR 250°C''', '''t=780 sec'''

⚫
Cleaning recipe name: '''Post dep PD''', '''t=900sec'''


d) Run the job (name the job/select the wafer, execute the job)
d) Run the job (name the job/select the wafer, execute the job)


You can repeat the previous step for each wafer. This way after loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.


⚫
e) Unload wafers '''ONLY''' when all runs are finished.
⚫
·     There is '''only one SiO2 seasoning recipe''' that is used for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.


⚫
=== '''Unaxis deposition - 300nm SiO2 HDR film @250°C''' ===
⚫
e) Unload wafers ONLY when all runs are finished.

⚫
=== '''2. Unaxis SiO2 HDR @250°C deposition''' ===
a) Prepare three 4” wafers:
a) Prepare three 4” wafers:
⚫
* for seasoning (regular Si wafer ~500nm thick)

⚫
* for deposition (your wafer for deposition)
⚫
·     for seasoning (regular Si wafer ~500nmthick)
⚫
* for cleaning ( Si thick wafer~0.8-1um )

⚫
·     for deposition (your wafer for deposition)

⚫
·     for cleaning ( Si thick wafer~0.8-1um )

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.


c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in the recipe.
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in recipes.
⚫
* Seasoning recipe name: '''SiO2 seasoning, t=2min'''

Seasoning recipe name: '''SiO2 seasoning, t=2min'''
* Deposition recipe name: '''SiO2 HDR 250°C''', '''t=180 sec'''
⚫
* Cleaning recipe name: '''Post dep PD''', '''t=900sec'''

⚫
There is '''only one SiO2 seasoning''' recipe. This same recipe is used for seasoning for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.
⚫
Deposition recipe name: '''SiO2 HDR 250°C''', '''t=180 sec'''

⚫
Cleaning recipe name: '''Post dep PD''', '''t=900sec'''


d) Run the job (name the job/select the wafer, execute the job)
d) Run the job (name the job/select the wafer, execute the job)


You can repeat the previous step for each wafer. This way after loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.


⚫
e) Unload wafers '''ONLY''' when all runs are finished.
⚫
·     There is '''only one SiO2 seasoning recipe''' that is used for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.


⚫
=== '''Unaxis deposition - 300nm SiN film @250°C''' ===
⚫
e) Unload wafers ONLY when all runs are finished.

⚫
=== '''3. Unaxis SiN @250°C deposition''' ===
a) Prepare three 4” wafers:
a) Prepare three 4” wafers:
⚫
* for seasoning (regular Si wafer ~500nm thick)

⚫
* for deposition (your wafer for deposition)
⚫
·     for seasoning (regular Si wafer ~500nmthick)
⚫
* for cleaning ( Si thick wafer~0.8-1um)

⚫
·     for deposition (your wafer for deposition)

⚫
·     for cleaning ( Si thick wafer~0.8-1um)

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.


c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in the recipe.
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in recipes.
⚫
* Seasoning recipe name: '''SiN seasoning''', '''t=5min'''

Seasoning recipe name: '''SiN seasoning''', '''t=5min'''
* Deposition recipe name: '''SiN 250°C, t=480 sec'''
⚫
* Cleaning recipe name: '''Post dep PD,''' '''t=1500sec'''

⚫
Deposition recipe name: '''SiN 250°C, t=480 sec'''

⚫
Cleaning recipe name: '''Post dep PD,''' '''t=1500sec'''

d) Run the job (name the job/select the wafer, execute the job)
d) Run the job (name the job/select the wafer, execute the job)


You can repeat the previous step for each wafer. This way after loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.


e) Unload wafers ONLY when all runs are finished.
e) Unload wafers '''ONLY''' when all runs are finished.


=== 4. '''Unaxis SiN LS @250°C''' '''deposition''' ===
=== '''Unaxis deposition - 300nm SiN LS film @250°C''' ===
a) Prepare three 4”wafers:
a) Prepare three 4”wafers:
* for seasoning (regular Si wafer ~500nm thick)

⚫
* for deposition (your wafer for deposition)
⚫
·     for seasoning (regular Si wafer ~500nmthick)
⚫
* for cleaning ( Si thick wafer~0.8-1um )

·     for deposition (your wafer for deposition)

⚫
·     for cleaning ( Si thick wafer~0.8-1um )

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.


c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in the recipe.
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in recipes.
⚫
* Seasoning recipe name: '''SiN seasoning''', '''t=2min'''

Seasoning recipe name: '''SiN seasoning''', '''t=2min'''
* Deposition recipe name: '''SiN LS''' '''250°C''', '''t=180 sec'''
⚫
* Cleaning recipe name: '''Post dep PD,''' '''t=1500sec'''

⚫
Deposition recipe name: '''SiN LS''' '''250°C''', '''t=180 sec'''

⚫
Cleaning recipe name: '''Post dep PD,''' '''t=1500sec'''

d) Run the job (name the job/select the wafer, execute the job)
d) Run the job (name the job/select the wafer, execute the job)


You can repeat the previous step for each wafer. This way after loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.


e) Unload wafers ONLY when all runs are finished.
e) Unload wafers '''ONLY''' when all runs are finished.

Latest revision as of 20:32, 30 March 2020

Unaxis deposition - 300nm SiO2 LDR film @250°C

a) Prepare three 4” wafers:

  • for seasoning (regular Si wafer ~500nm thick)
  • for deposition (your wafer for deposition)
  • for cleaning ( Si thick wafer~0.8-1um)

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.

c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes.

  • Seasoning recipe name: SiO2 seasoning, t=2min
  • Deposition recipe name: SiO2 LDR 250°C, t=780 sec
  • Cleaning recipe name: Post dep PD, t=900sec

There is only one SiO2 seasoning recipe. This same recipe is used for seasoning for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.

d) Run the job (name the job/select the wafer, execute the job)

After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.

e) Unload wafers ONLY when all runs are finished.

Unaxis deposition - 300nm SiO2 HDR film @250°C

a) Prepare three 4” wafers:

  • for seasoning (regular Si wafer ~500nm thick)
  • for deposition (your wafer for deposition)
  • for cleaning ( Si thick wafer~0.8-1um )

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.

c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes.

  • Seasoning recipe name: SiO2 seasoning, t=2min
  • Deposition recipe name: SiO2 HDR 250°C, t=180 sec
  • Cleaning recipe name: Post dep PD, t=900sec

There is only one SiO2 seasoning recipe. This same recipe is used for seasoning for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.

d) Run the job (name the job/select the wafer, execute the job)

After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.

e) Unload wafers ONLY when all runs are finished.

Unaxis deposition - 300nm SiN film @250°C

a) Prepare three 4” wafers:

  • for seasoning (regular Si wafer ~500nm thick)
  • for deposition (your wafer for deposition)
  • for cleaning ( Si thick wafer~0.8-1um)

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.

c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes.

  • Seasoning recipe name: SiN seasoning, t=5min
  • Deposition recipe name: SiN 250°C, t=480 sec
  • Cleaning recipe name: Post dep PD, t=1500sec

d) Run the job (name the job/select the wafer, execute the job)

After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.

e) Unload wafers ONLY when all runs are finished.

Unaxis deposition - 300nm SiN LS film @250°C

a) Prepare three 4”wafers:

  • for seasoning (regular Si wafer ~500nm thick)
  • for deposition (your wafer for deposition)
  • for cleaning ( Si thick wafer~0.8-1um )

b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.

c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes.

  • Seasoning recipe name: SiN seasoning, t=2min
  • Deposition recipe name: SiN LS 250°C, t=180 sec
  • Cleaning recipe name: Post dep PD, t=1500sec

d) Run the job (name the job/select the wafer, execute the job)

After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run.

e) Unload wafers ONLY when all runs are finished.