There are three standard recipes : STD SiO2, STD Nitride2, and STD LS Nitride2 at 300C. Instructions bellow explain how to run each of the recipes ( seasoning, deposition, cleaning) |
|||
=== Unaxis deposition - 300nm SiO2 LDR film @250°C === |
|||
a) Prepare three 4” wafers: |
|||
* for seasoning (regular Si wafer ~500nm thick) |
|||
* for deposition (your wafer for deposition) |
|||
* for cleaning ( Si thick wafer~0.8-1um) |
|||
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers. |
|||
=== Standard Oxide Deposition === |
|||
c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes. |
|||
* Seasoning recipe name: SiO2 seasoning, t=2min |
|||
* Deposition recipe name: SiO2 LDR 250°C, t=780 sec |
|||
* Cleaning recipe name: Post dep PD, t=900sec |
|||
There is only one SiO2 seasoning recipe. This same recipe is used for seasoning for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls. |
|||
==== STD SiO v2 ==== |
|||
d) Run the job (name the job/select the wafer, execute the job) |
|||
#Log in to Advanced PECVD #2 |
|||
#Seasoning |
|||
#*Load the seasoning recipe (STD SiO v2). Edit deposition time to 10min and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition. |
|||
#Deposition |
|||
#*Vent the chamber and load the substrate (place it in the center of platen). You can place glass slides around the wafer to protect it from moving. |
|||
#*Pump down. |
|||
#*Load the deposition recipe (STD SiO v2). Edit deposition time to desired time and run it. Deposition time is variable. Get the rate from [https://wiki.nanotech.ucsb.edu/wiki/PECVD_Recipes#PECVD_2_.28Advanced_Vacuum.29 historical data]. |
|||
#*Unload the wafer. |
|||
#Cleaning |
|||
#*Wet clean: Wipe sidewall first with DI water, followed by IPA (Do wet clean only if [coat+deposition] time was >29min]). |
|||
#*Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning [one minute clean for one minute [coat+deposition] time. |
|||
#*Log out |
|||
=== Standard Nitride Deposition === |
|||
==== "STD Si3N4 v3" ==== |
|||
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run. |
|||
#Log in to Advanced PECVD #2 |
|||
#Seasoning |
|||
#*Load the seasoning recipe (STD Si3N4 v3). Edit deposition time to 10min and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition. |
|||
#Deposition |
|||
#*Vent the chamber and load the substrate (place it in the center of platen). You can place glass slides around the wafer to protect it from moving. |
|||
#*Pump down. |
|||
#*Load the deposition recipe (STD Si3N4 v3). Edit deposition time to desired time and run it. Deposition time is variable. Get the rate from [https://wiki.nanotech.ucsb.edu/wiki/PECVD_Recipes#PECVD_2_.28Advanced_Vacuum.29 historical data]. |
|||
#*Unload the wafer. |
|||
#Cleaning |
|||
#*Wet clean: Wipe sidewall first with DI water, followed by IPA (Do wet clean only if [coat+deposition] time was >29min]). |
|||
#*Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning [(coat time+deposition time)/7]. |
|||
#*Log out |
|||
=== Standard Low Stress Nitride Deposition === |
|||
e) Unload wafers ONLY when all runs are finished. |
|||
==== "STD LS-Si3N4 v4" ==== |
|||
=== Unaxis deposition - 300nm SiO2 HDR film @250°C === |
|||
#Log in to Advanced PECVD #2 |
|||
a) Prepare three 4” wafers: |
|||
#Seasoning |
|||
* for seasoning (regular Si wafer ~500nm thick) |
|||
#*Load the seasoning recipe (STD LS-Si3N4 v4). Edit deposition time to 10min and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition. |
|||
* for deposition (your wafer for deposition) |
|||
#Deposition |
|||
* for cleaning ( Si thick wafer~0.8-1um ) |
|||
#*Vent the chamber and load the substrate (place it in the center of platen). You can place small glass slides round the wafer to protect it from moving. |
|||
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers. |
|||
#*Pump down. |
|||
#*Load the deposition recipe (STD LS-Si3N4 v4). Edit deposition time to desired time and run it. Get the rate from [https://wiki.nanotech.ucsb.edu/wiki/PECVD_Recipes#PECVD_2_.28Advanced_Vacuum.29 historical data]. |
|||
c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes. |
|||
#*Make sure Loop is set correctly for HF/LF Process Step |
|||
* Seasoning recipe name: SiO2 seasoning, t=2min |
|||
#*Unload the wafer. |
|||
* Deposition recipe name: SiO2 HDR 250°C, t=180 sec |
|||
#Cleaning |
|||
* Cleaning recipe name: Post dep PD, t=900sec |
|||
#*Wet clean: Wipe sidewall first with DI water, followed by IPA (Do wet clean only if [coat+deposition] time was >29min]). |
|||
There is only one SiO2 seasoning recipe. This same recipe is used for seasoning for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls. |
|||
#*Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning [(coat time+deposition time)/7]. |
|||
#*Log out |
|||
d) Run the job (name the job/select the wafer, execute the job) |
|||
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run. |
|||
e) Unload wafers ONLY when all runs are finished. |
|||
=== Unaxis deposition - 300nm SiN film @250°C === |
|||
a) Prepare three 4” wafers: |
|||
* for seasoning (regular Si wafer ~500nm thick) |
|||
* for deposition (your wafer for deposition) |
|||
* for cleaning ( Si thick wafer~0.8-1um) |
|||
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers. |
|||
c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes. |
|||
* Seasoning recipe name: SiN seasoning, t=5min |
|||
* Deposition recipe name: SiN 250°C, t=480 sec |
|||
* Cleaning recipe name: Post dep PD, t=1500sec |
|||
d) Run the job (name the job/select the wafer, execute the job) |
|||
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run. |
|||
e) Unload wafers ONLY when all runs are finished. |
|||
=== Unaxis deposition - 300nm SiN LS film @250°C === |
|||
a) Prepare three 4”wafers: |
|||
* for seasoning (regular Si wafer ~500nm thick) |
|||
* for deposition (your wafer for deposition) |
|||
* for cleaning ( Si thick wafer~0.8-1um ) |
|||
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers. |
|||
c) Edit standard recipes (for seasoning, deposition, and cleaning). You can ONLY change the time in recipes. |
|||
* Seasoning recipe name: SiN seasoning, t=2min |
|||
* Deposition recipe name: SiN LS 250°C, t=180 sec |
|||
* Cleaning recipe name: Post dep PD, t=1500sec |
|||
d) Run the job (name the job/select the wafer, execute the job) |
|||
After loading the wafers and selecting for each wafer correct recipe, you could leave and come back when all runs are finished. You should monitor process at the very beginning to make sure there are no any issues with the run. |
|||
e) Unload wafers ONLY when all runs are finished. |
|||
Latest revision as of 23:12, 19 February 2025
There are three standard recipes : STD SiO2, STD Nitride2, and STD LS Nitride2 at 300C. Instructions bellow explain how to run each of the recipes ( seasoning, deposition, cleaning)
Standard Oxide Deposition
STD SiO v2
- Log in to Advanced PECVD #2
- Seasoning
- Load the seasoning recipe (STD SiO v2). Edit deposition time to 10min and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place glass slides around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (STD SiO v2). Edit deposition time to desired time and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wet clean: Wipe sidewall first with DI water, followed by IPA (Do wet clean only if [coat+deposition] time was >29min]).
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning [one minute clean for one minute [coat+deposition] time.
- Log out
Standard Nitride Deposition
"STD Si3N4 v3"
- Log in to Advanced PECVD #2
- Seasoning
- Load the seasoning recipe (STD Si3N4 v3). Edit deposition time to 10min and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place glass slides around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (STD Si3N4 v3). Edit deposition time to desired time and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wet clean: Wipe sidewall first with DI water, followed by IPA (Do wet clean only if [coat+deposition] time was >29min]).
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning [(coat time+deposition time)/7].
- Log out
Standard Low Stress Nitride Deposition
"STD LS-Si3N4 v4"
- Log in to Advanced PECVD #2
- Seasoning
- Load the seasoning recipe (STD LS-Si3N4 v4). Edit deposition time to 10min and run it. The goal of this step is to coat oxide on chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place small glass slides round the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (STD LS-Si3N4 v4). Edit deposition time to desired time and run it. Get the rate from historical data.
- Make sure Loop is set correctly for HF/LF Process Step
- Unload the wafer.
- Cleaning
- Wet clean: Wipe sidewall first with DI water, followed by IPA (Do wet clean only if [coat+deposition] time was >29min]).
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning [(coat time+deposition time)/7].
- Log out