Created page with "'''PECVD#1 deposition - 300nm SiN film @250°C''' The wafers are ordered from SVM. These are low particle count 4" Si wafer where particle count is very low <100. a)Log in to..." |
No edit summary |
||
(5 intermediate revisions by the same user not shown) | |||
Line 1: | Line 1: | ||
[[Table SiO2 recipe]] |
|||
'''PECVD#1 deposition - 300nm SiN film @250°C''' |
|||
The wafers are ordered from SVM. These are low particle count 4" Si wafer where particle count is very low <100. |
|||
a)Log in to PECVD #1 (Staff account) |
|||
b)Edit standard recipes (for seasoning, deposition, and cleaning). You can '''ONLY''' change the time in recipes. |
|||
• Seasoning recipe name: |
|||
• Deposition recipe name: |
|||
• Cleaning recipe name: |
|||
c)Load the recipe for seasoning, and run it. The goal of this step is to coat chamber walls and prepare it for deposition. |
|||
d)Vent the chamber and load 4"Si wafer (place in in the center of platen). You can place small pieces around, to protect wafer from moving |
|||
e)Pump down and load the recipe for deposition. |
|||
f) Edit the recipe for deposition, change the time ONLY. |
|||
d) Run deposition |
|||
e) Unload wafer |
|||
f) Wipe sidewall first with wafter then with IPA. |
|||
g) Load recipe for cleaning. Edit the recipe and etner required time for cleaning. |
|||
h)Run the cleaning |