|1/11/23 |
|||
|ND_Pan2_011123 |
|||
|142.9 |
|||
|1.11 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/1/18/30_pan2_011123_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/e/eb/Cs_pan2_011123_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|12/15/22 |
|||
|ND_Pan2_121522 |
|||
|148 |
|||
|1.10 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/a/a8/30D_pan2_121522_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/3/33/CS_pan2_121522_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|12/09/22 |
|||
|ND_Pan2_120922 |
|||
|138 |
|||
|1.12 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/b/b3/30D_pan2_120922_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/9/99/CS_pan2_120922_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|11/18/22 |
|||
|ND_Pan2_111822 |
|||
|154 |
|||
|1.33 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/8/82/30D_pan2_111822_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/c/c9/CS_pan2_111822_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|11/07/22 |
|||
|ND_Pan2_110722 |
|||
|155.7 |
|||
|1.18 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/f/f1/30D_pan2_110722_002.jpg <nowiki>[30]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/4/43/CS_pan2_110722_003.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|10/21/22 |
|||
|ND_Pan2_102122 |
|||
|148.6 |
|||
|1.37 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/f/f5/30D_pan2_102122_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/3/3d/CS_pan2_102122_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|10/10/22 |
|||
|ND_Pan2_101022 |
|||
|118.3 |
|||
|1.07 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/7/7c/30D_pan2_101022_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/9/9b/CS_pan2_101022_003.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|10/3/22 |
|||
|ND_Pan2_100322 |
|||
|143.1 |
|||
|1.23 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/a/a0/30D_10302022_pan2_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/6/6d/CS_10302022_pan2_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|9/26/22 |
|||
|ND_Pan2n_092622 |
|||
|131.4 |
|||
|1.40 |
|||
|Samples from new wafer |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/b/b4/30D_Pan2n_092622_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/c/c7/CS_Pan1n_092622_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|9/26/22 |
|||
|ND_Pan2o_092622 |
|||
|130.6 |
|||
|1.14 |
|||
|Samples from old wafer |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/7/79/45D_Pan2o_092622_002.jpg <nowiki>[45D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/8/8e/CS_Pan2n_092622_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|9/12/22 |
|||
|ND_Pan2_091222 |
|||
|156 |
|||
|1.33 |
|||
|Higher etch rate/selectivity, may be due to new Si wafer |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/7/79/30D_pan2_091222_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/c/cf/CS_pan2_091222_002.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|8/26/22 |
|||
|ND_Pan2_082622 |
|||
|144.3 |
|||
|1.22 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/7/71/30D_Pan2_082622_001.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/a/ad/CS_Pan2_082622_001.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|8/8/2022 |
|||
|ND_Pan2_080822 |
|||
|134.3 |
|||
|1.12 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/6/6d/30D_08082022_pan2_001.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/c/c0/CS_08082022_pan2_001.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|||
|7/29/2022 |
|||
|ND_Pan2_072922 |
|||
|142.3 |
|||
|1.20 |
|||
| |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/e/ef/30D_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/d/db/CS_002_07-29-22.jpg <nowiki>[CS]</nowiki>] |
|||
|- |
|- |
||
|7/15/2022 |
|7/15/2022 |
||
| Line 15: | Line 113: | ||
|1.20 |
|1.20 |
||
| |
| |
||
|[https://wiki.nanotech.ucsb.edu/w/images/a/a5/ND_Pan2_071522_45D.jpg <nowiki>[45D]</nowiki>] |
|[https://wiki.nanotech.ucsb.edu/w/images/a/a5/ND_Pan2_071522_45D.jpg <nowiki>[45D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/f/fe/ND_Pan2_071522_CS.jpg <nowiki>[CS]</nowiki>] |
||
|- |
|- |
||
|5/5/2022 |
|5/5/2022 |
||
| Line 21: | Line 119: | ||
|170 |
|170 |
||
|1.11 |
|1.11 |
||
|Right after Quartz Top-Plate Temperature reduced 100°C-->50°C |
|Right after Quartz Top-Plate Temperature reduced 100°C-->50°C. |
||
Etch Characteristics look similar to before. |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/9/94/ICP2_07_45D_002.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/1/10/ICP2_07_CS_005.jpg <nowiki>[2]</nowiki>] |
|[https://wiki.nanotech.ucsb.edu/w/images/9/94/ICP2_07_45D_002.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/1/10/ICP2_07_CS_005.jpg <nowiki>[2]</nowiki>] |
||
|- |
|- |
||
| Line 70: | Line 169: | ||
|140 |
|140 |
||
|0.97 |
|0.97 |
||
|After etching diamond sample for 1 hour using Cl2/Ar. Found |
|After etching diamond sample for 1 hour using Cl2/Ar. Found |
||
chamber/etches are ok. |
|||
|[https://wiki.nanotech.ucsb.edu/w/images/2/26/I2210508.pdf] |
|[https://wiki.nanotech.ucsb.edu/w/images/2/26/I2210508.pdf] |
||
|- |
|- |
||
Latest revision as of 20:15, 11 January 2023
| ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec | |||||
| Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Comments | SEM Images; |
|---|---|---|---|---|---|
| 1/11/23 | ND_Pan2_011123 | 142.9 | 1.11 | [30D][CS] | |
| 12/15/22 | ND_Pan2_121522 | 148 | 1.10 | [30D][CS] | |
| 12/09/22 | ND_Pan2_120922 | 138 | 1.12 | [30D][CS] | |
| 11/18/22 | ND_Pan2_111822 | 154 | 1.33 | [30D][CS] | |
| 11/07/22 | ND_Pan2_110722 | 155.7 | 1.18 | [30] [CS] | |
| 10/21/22 | ND_Pan2_102122 | 148.6 | 1.37 | [30D] [CS] | |
| 10/10/22 | ND_Pan2_101022 | 118.3 | 1.07 | [30D] [CS] | |
| 10/3/22 | ND_Pan2_100322 | 143.1 | 1.23 | [30D] [CS] | |
| 9/26/22 | ND_Pan2n_092622 | 131.4 | 1.40 | Samples from new wafer | [30D] [CS] |
| 9/26/22 | ND_Pan2o_092622 | 130.6 | 1.14 | Samples from old wafer | [45D] [CS] |
| 9/12/22 | ND_Pan2_091222 | 156 | 1.33 | Higher etch rate/selectivity, may be due to new Si wafer | [30D] [CS] |
| 8/26/22 | ND_Pan2_082622 | 144.3 | 1.22 | [30D] [CS] | |
| 8/8/2022 | ND_Pan2_080822 | 134.3 | 1.12 | [30D] [CS] | |
| 7/29/2022 | ND_Pan2_072922 | 142.3 | 1.20 | [30D] [CS] | |
| 7/15/2022 | ND_Pan2_071522 | 139.1 | 1.20 | [45D][CS] | |
| 5/5/2022 | NP_ICP2_07 | 170 | 1.11 | Right after Quartz Top-Plate Temperature reduced 100°C-->50°C.
Etch Characteristics look similar to before. |
[1] [2] |
| 4/26/2022 | NP_ICP2_06 | 176.3 | 1.14 | [1] [2] | |
| 4/20/2022 | NP_ICP2_05 | 171.7 | 1.13 | [1] [2] | |
| 4/12/2022 | NP_ICP2_04 | 167.9 | 1.17 | [1] [2] | |
| 3/30/2022 | NP_ICP2_03 | 164 | 1.23 | [1] [2] | |
| 3/8/2022 | NP_ICP2_02 | 144 | 1.02 | [1] [2] | |
| 3/2/2022 | NP_ICP2_01 | 169.6 | 1.29 | [1] [2] | |
| 8/9/2021 | I22105 | 140 | 0.97 | After etching diamond sample for 1 hour using Cl2/Ar. Found
chamber/etches are ok. |
[1] |
| 8/9/2021 | I22104 | 147 | 1.06 | Before etching diamond sample for 1 hour using Cl2/Ar | [2] |
| 7/21/2021 | I22103 | 134 | 1.09 | Investigating reports of low etch rate | [3] |
| 5/19/2021 | I22102 | 163 | 1.11 | Etch time=130 sec | [4] |
| 1/7/2021 | I22101 | 144 | 1.20 | [5] | |
| 8/9/2020 | I22002 | 102 | 0.86 | caused by air leaking to CHF3 channel | [6] |
| 1/16/2020 | I22001 | 149 | 1.21 | [7] | |
| 7/18/2019 | I21905 | 162 | 1.37 | [8] | |
| 3/6/2019 | I21904 | 151 | 1.23 | 85.6 | [9] |
| 1/28/2019 | I21901 | 146 | 1.23 | [10] | |
| 10/5/2018 | SiO2#02 | 160 | 1.2 | 82.1 | [11] |
Alternate Data (not updated)