Thermal Evap 2 (Solder): Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
| (42 intermediate revisions by 5 users not shown) | |||
| Line 1: | Line 1: | ||
{{ |
{{tool2|{{PAGENAME}} |
||
|picture=Thermal2.jpg |
|picture=Thermal2.jpg |
||
|type = Vacuum Deposition |
|type = Vacuum Deposition |
||
|super= |
|super= Michael Barreraz |
||
|super2= Don Freeborn |
|||
|location=Bay 3 |
|location=Bay 3 |
||
|description = ? |
|description = ? |
||
| Line 10: | Line 11: | ||
}} |
}} |
||
= About = |
== About == |
||
Thermal evaporator #2 is the designated "Solder" evaporator. The tool is used primarily for solder materials including Gold, Indium and Tin. See the Recipes section below for other materials used. |
|||
Use this tool for materials with low melting temperatures, or for materials that have a high risk of contamination in the e-beam evaporators. |
|||
= Materials Table = |
|||
== Detailed Specifications == |
|||
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable" |
|||
Wafers up to 12" can be mounted. |
|||
|- |
|||
! colspan=6 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table</div> |
|||
==Documentation== |
|||
|- bgcolor="#D0E7FF" |
|||
*[//wiki.nanotech.ucsb.edu/w/images/b/b3/Thermal_Evaporator2.pdf Operating Instructions] |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Material''' |
|||
*[https://wiki.nanofab.ucsb.edu/w/images/1/17/Thermal_Evaporator2-Normal_Fixture-_Indium_Deposition.pdf Using Normal Fixture] |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Symbol''' |
|||
*[https://wiki.nanofab.ucsb.edu/w/images/d/d1/Thermal_Evaprator2-Cold_Fixture-Indium_Deposition.pdf Using Cold Fixture] |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Density, g/cm3''' |
|||
*[https://wiki.nanofab.ucsb.edu/w/images/7/74/Thermal_Evap_2_pump_down_procedure-New-_5-29-25.pdf Temp Pump Down SOP as of 5-29-25] |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Z Ratio''' |
|||
! width="45" bgcolor="#D0E7FF" align="center" | '''Tooling, %''' |
|||
== Recipes == |
|||
! width="100" bgcolor="#D0E7FF" align="center" | '''Comments''' |
|||
* [[Thermal Evaporation Recipes#Thermal Evaporator 2|Recipes > Thermal Evaporation Recipes > Thermal Evaporator 2]] |
|||
|- |
|||
** ''Visit this page for the materials table and evaporation parameters for all materials available.'' |
|||
|Aluminum |
|||
* [https://wiki.nanofab.ucsb.edu/w/images/0/05/Sn_deposition_in_Thermal_Evaporator2.pdf Tin deposition] |
|||
|Al |
|||
|2.70 |
|||
== Plot == |
|||
|1.08 |
|||
* [https://wiki.nanofab.ucsb.edu/w/images/b/bb/Thermal_Evaporator2-Plot.png Plot for Indium Deposition] |
|||
| |
|||
| |
|||
|- |
|||
|Antimony |
|||
|Sb |
|||
|2.70 |
|||
|0.768 |
|||
| |
|||
| |
|||
|- |
|||
|Arsenic |
|||
|As |
|||
|5.73 |
|||
|0.996 |
|||
| |
|||
| |
|||
|- |
|||
|Beryllium |
|||
|Be |
|||
|1.85 |
|||
|0.543 |
|||
| |
|||
| |
|||
|- |
|||
|Boron |
|||
|B |
|||
|2.54 |
|||
|0.389 |
|||
| |
|||
| |
|||
|- |
|||
|Cadmium |
|||
|Cd |
|||
|8.64 |
|||
|0.682 |
|||
| |
|||
| |
|||
|- |
|||
|Cadmium sulfide |
|||
|CdS |
|||
|4.83 |
|||
|1.02 |
|||
| |
|||
| |
|||
|- |
|||
|Cadmium telluride |
|||
|CdTe |
|||
|5.85 |
|||
|0.980 |
|||
| |
|||
| |
|||
|- |
|||
|Calcium fluoride |
|||
|CaF<sub>2</sub> |
|||
|3.18 |
|||
|0.775 |
|||
| |
|||
| |
|||
|- |
|||
|Carbon (graphite) |
|||
|C |
|||
|2.25 |
|||
|3.26 |
|||
| |
|||
| |
|||
|- |
|||
|Chromium |
|||
|Cr |
|||
|7.20 |
|||
|0.305 |
|||
|155 |
|||
| |
|||
|- |
|||
|Cobalt |
|||
|Co |
|||
|8.71 |
|||
|0.343 |
|||
| |
|||
| |
|||
|- |
|||
|Copper |
|||
|Cu |
|||
|8.93 |
|||
|0.437 |
|||
| |
|||
| |
|||
|- |
|||
|Gallium |
|||
|Ga |
|||
|5.93 |
|||
|0.593 |
|||
| |
|||
| |
|||
|- |
|||
|Gallium Arsenide |
|||
|GaAs |
|||
|5.31 |
|||
|1.59 |
|||
| |
|||
| |
|||
|- |
|||
|Germanium |
|||
|Ge |
|||
|5.35 |
|||
|0.516 |
|||
| |
|||
| |
|||
|- |
|||
|Gold |
|||
|Au |
|||
|19.30 |
|||
|0.381 |
|||
| |
|||
|Used often |
|||
|- |
|||
|Indium |
|||
|In |
|||
|7.30 |
|||
|0.841 |
|||
|120 |
|||
| |
|||
|- |
|||
|Indium antimonide |
|||
|InSb |
|||
|5.76 |
|||
|0.769 |
|||
| |
|||
| |
|||
|- |
|||
|Iridium |
|||
|Ir |
|||
|22.4 |
|||
|0.129 |
|||
| |
|||
| |
|||
|- |
|||
|Iron |
|||
|Fe |
|||
|7.86 |
|||
|0.349 |
|||
| |
|||
| |
|||
|- |
|||
|Lead |
|||
|Pb |
|||
|11.3 |
|||
|1.13 |
|||
| |
|||
| |
|||
|- |
|||
|Lead sulfide |
|||
|PbS |
|||
|7.50 |
|||
|0.566 |
|||
| |
|||
| |
|||
|- |
|||
|Lithium fluoride |
|||
|LiF |
|||
|2.64 |
|||
|0.774 |
|||
| |
|||
| |
|||
|- |
|||
|Magnesium |
|||
|Mg |
|||
|1.74 |
|||
|1.61 |
|||
| |
|||
| |
|||
|- |
|||
|Magnesium oxide |
|||
|MgO |
|||
|3.58 |
|||
|0.411 |
|||
| |
|||
| |
|||
|- |
|||
|Magnesium Fluoride |
|||
|MgF<sub>2</sub> |
|||
|3.00 |
|||
|0.427 |
|||
| |
|||
| |
|||
|- |
|||
|Manganese |
|||
|Mn |
|||
|7.20 |
|||
|0.377 |
|||
| |
|||
| |
|||
|- |
|||
|Manganese(II) Sulfide |
|||
|MnS |
|||
|3.99 |
|||
|0.94 |
|||
| |
|||
| |
|||
|- |
|||
|Mercury |
|||
|Hg |
|||
|13.46 |
|||
|0.74 |
|||
| |
|||
| |
|||
|- |
|||
|Molybdenum |
|||
|Mo |
|||
|10.2 |
|||
|0.257 |
|||
| |
|||
| |
|||
|- |
|||
|Nickel |
|||
|Ni |
|||
|8.91 |
|||
|0.331 |
|||
| |
|||
| |
|||
|- |
|||
|Niobium |
|||
|Nb |
|||
|8.57 |
|||
|0.493 |
|||
| |
|||
| |
|||
|- |
|||
|Niobium(V) Oxide |
|||
|Nb<sub>2</sub>O<sub>5</sub> |
|||
|4.47 |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
|Palladium |
|||
|Pd |
|||
|12.0 |
|||
|0.357 |
|||
| |
|||
| |
|||
|- |
|||
|Platinum |
|||
|Pt |
|||
|21.4 |
|||
|0.245 |
|||
| |
|||
| |
|||
|- |
|||
|Potasium Cloride |
|||
|KCl |
|||
|1.98 |
|||
|2.05 |
|||
| |
|||
| |
|||
|- |
|||
|Selenium |
|||
|Se |
|||
|4.82 |
|||
|0.864 |
|||
| |
|||
| |
|||
|- |
|||
|Silicon |
|||
|Si |
|||
|2.32 |
|||
|0.712 |
|||
| |
|||
| |
|||
|- |
|||
|Silicon(II) Oxide |
|||
|SiO |
|||
|2.13 |
|||
|0.87 |
|||
| |
|||
| |
|||
|- |
|||
|Silicon dioxide (fused quarz) |
|||
|SiO<sub>2</sub> |
|||
|2.20 |
|||
|1.07 |
|||
| |
|||
| |
|||
|- |
|||
|Silver |
|||
|Ag |
|||
|10.5 |
|||
|0.529 |
|||
| |
|||
| |
|||
|- |
|||
|Silver bromide |
|||
|AgBr |
|||
|6.47 |
|||
|1.18 |
|||
| |
|||
| |
|||
|- |
|||
|Silver chloride |
|||
|AgCl |
|||
|5.56 |
|||
|1.32 |
|||
| |
|||
| |
|||
|- |
|||
|Sodium |
|||
|Na |
|||
|0.97 |
|||
|4.8 |
|||
| |
|||
| |
|||
|- |
|||
|Sodium chloride |
|||
|NaCl |
|||
|2.17 |
|||
|1.57 |
|||
| |
|||
| |
|||
|- |
|||
|Tantalum |
|||
|Ta |
|||
|16.6 |
|||
|0.262 |
|||
| |
|||
| |
|||
|- |
|||
|Tantalum(IV) oxide |
|||
|Ta<sub>2</sub>O<sub>5</sub> |
|||
|8.2 |
|||
|0.30 |
|||
| |
|||
| |
|||
|- |
|||
|Tin |
|||
|Sn |
|||
|7.30 |
|||
|0.724 |
|||
| |
|||
| |
|||
|- |
|||
|Titanium |
|||
|Ti |
|||
|4.50 |
|||
|0.628 |
|||
| |
|||
| |
|||
|- |
|||
|Titanium (IV) Oxide |
|||
|TiO<sub>2</sub> |
|||
|4.26 |
|||
|0.40 |
|||
| |
|||
| |
|||
|- |
|||
|Titanium Oxide |
|||
|TiO |
|||
|4.90 |
|||
|N/A |
|||
| |
|||
| |
|||
|- |
|||
|Tangsten |
|||
|W |
|||
|19.3 |
|||
|0.163 |
|||
| |
|||
| |
|||
|- |
|||
|Tangsten carbide |
|||
|WC |
|||
|15.6 |
|||
|0.151 |
|||
| |
|||
| |
|||
|- |
|||
|Zinc |
|||
|Zn |
|||
|7.04 |
|||
|0.514 |
|||
| |
|||
| |
|||
|- |
|||
|Zinc Oxide |
|||
|Zn |
|||
|5.61 |
|||
|0.556 |
|||
| |
|||
| |
|||
|- |
|||
|Zinc Sulfide |
|||
|ZnS |
|||
|4.09 |
|||
|0.775 |
|||
| |
|||
| |
|||
|- |
|||
|Zirconium |
|||
|Zr |
|||
|6.51 |
|||
|0.60 |
|||
| |
|||
| |
|||
|- |
|||
|Zirconium Oxide |
|||
|ZrO<sub>2</sub> |
|||
|5.6 |
|||
| |
|||
| |
|||
| |
|||
|- |
|||
Latest revision as of 21:35, 19 June 2025
| ||||||||||||||||||||||||||||||
About
Thermal evaporator #2 is the designated "Solder" evaporator. The tool is used primarily for solder materials including Gold, Indium and Tin. See the Recipes section below for other materials used.
Use this tool for materials with low melting temperatures, or for materials that have a high risk of contamination in the e-beam evaporators.
Detailed Specifications
Wafers up to 12" can be mounted.
Documentation
Recipes
- Recipes > Thermal Evaporation Recipes > Thermal Evaporator 2
- Visit this page for the materials table and evaporation parameters for all materials available.
- Tin deposition