Atomic Layer Deposition Recipes: Difference between revisions
No edit summary |
|||
| (57 intermediate revisions by 5 users not shown) | |||
| Line 1: | Line 1: | ||
{{recipes|Vacuum Deposition}} |
{{recipes|Vacuum Deposition}} |
||
=[[Atomic Layer Deposition (Oxford FlexAL)]]= |
=[[Atomic Layer Deposition (Oxford FlexAL)]]= |
||
==Al{{sub|2}}O{{sub|3}} deposition (ALD)== |
|||
==Atomic Layer Deposition (aka ALD) - what is it?== |
|||
*{{fl|ALD-Al2O3-300-Recipe.pdf|Al{{sub|2}}O{{sub|3}} 300}} |
|||
Atomic layer deposition (ALD) utilizes sequential exposure cycles of 2 gaseous precursors to a substrate surface. Each half-cycle exposes one of the precursors to the substrate (and in the absence of the other) to ensure a "saturated" coverage on the surface. The saturation in exposure within each half-cycle leads to the self-limiting reaction behavior which defines an ALD process from other deposition techniques. With this in place, the deposition can proceed layer-by-layer with cycling and will result in uniform conformal growth over different substrate topographies. |
|||
*{{fl|ALD-Al2O3-300-Saturated-Recipe.pdf|Al{{sub|2}}O{{sub|3}} 300 Saturated}} |
|||
*{{fl|ALD-Al2O3-Plasma-300C-Recipe.pdf|Al{{sub|2}}O{{sub|3}} plasma 300C}} |
|||
*{{fl|ALD-Al2O3-100-Recipe.pdf|Al{{sub|2}}O{{sub|3}} 100}} |
|||
In most standard process, one half-cycle utilizes an organometallic precursor to deposit the metal of interest. The other half-cycle utilizes a counter-reactant to either oxidize or nitridize this metal to form the oxide or nitride film required. |
|||
==AlN deposition (ALD)== |
|||
*{{fl|ALD-AlN-300-recipe.pdf|AlN 300}} |
|||
By nature of the deposition process, the reactions are slow. <u>Hence, users are restricted to 30 nm maximum thickness for all films when using the tool.</u> Any deviations from this requirement needs special permission (contact [[Brian Lingg|Tool Supervisor]] if needed). |
|||
==HfO{{sub|2}} deposition (ALD)== |
|||
*{{fl|ALD-HfO2-100-recipe.pdf|HfO{{sub|2}} 100}} |
|||
*{{fl|ALD-HfO2-300-recipe.pdf|HfO{{sub|2}} 300}} |
|||
== Process Options == |
|||
==SiO{{sub|2}} deposition (ALD)== |
|||
*{{fl|ALD-SiO2-100-recipe.pdf|SiO{{sub|2}} 100}} |
|||
*{{fl|ALD-SiO2-300-recipe.pdf|SiO{{sub|2}} 300}} |
|||
== |
===Thermal ALD=== |
||
In all ALD processes used in our lab, the organometallic half-cycle is always thermal, i.e., the precursor is exposed to the substrate as a vapor. In a fully thermal ALD process, the counter reactant half-cycle also utilizes gas exposure to the substrate. Because the intact molecules are less reactive than activated gases from a plasma, thermal ALD can be on the slower side. One advantage however is this lower reactivity means that the substrate itself can remain inert to the deposition process. |
|||
*{{fl|ALD-ZrO2-300-recipe.pdf|ZrO{{sub|2}} 300}} |
|||
===Activated ALD=== |
|||
==== Plasma ==== |
|||
'''''O*''''' or '''''N*''''' in the recipe title means Oxygen or Nitrogen plasma, derived from flowing O2 or N2 gases through the ICP tube at the top of the chamber, respectively. |
|||
The plasma processes on this tool will run considerably faster than purely thermal processes, because the ions/radicals formed are significantly more reactive (which can be a drawback if depositing on a sensitive substrate). Note that the O* plasma can also reduce carbon contaminants from the organic precursors when forming oxide films. When growing nitride films, H2 is often added to the nitride-plasma gases to generate H* ions/radicals which can assist with the removal of C within the film. |
|||
==== Ozone ==== |
|||
'''''O3''''' in the recipe title refers to an oxidation reaction that uses an external Ozone generator for oxide growth (InUSA, Series 5000). Ozone is a more reactive form of oxygen than O2 that can be used to generate oxide films in a more thermal manner than plasma (which can sometimes be too aggressive). |
|||
Note that the generator must first be turned on prior to running any ozone-based recipe. Clicking on the O3 Generator icon on the tool desktop will open the control window. Both the O2 flow and the O3 concentration should be set to the defaults of 250 sccm and 19 wt% in the field settings. Clicking on the "Start Generator" button will start the ozone generator running. Wait for about 5 minutes for the system to stabilize. When done, <u>always</u> be sure to click on the "Stop Generator" button to turn off the generator and stop the O2 flow - it is very important not to forget to do this as the source could be burned out and/or the O2 bottle supplying the generator could be depleted if it runs too long! O2 will remain flowing for an additional minute to flush out any residual O3. Once that is completed, you can close the window. Check with [[Atomic Layer Deposition (Oxford FlexAL)|supervisor]] for further details. |
|||
==Chamber #1: Conductive Films== |
|||
Chamber 1 utilizes a dual manometer system that allows higher pressures during deposition than chamber 3. For example, chamber 1 has an upper limit of 2000 mTorr whereas chamber 3 has an upper limit of only 240 mTorr. The higher pressures allow the use of less reactive organo-metallic precursors to effect ALD growth in a reasonable time-frame. |
|||
'''Maximum 30nm deposition thickness for all processes in chamber 1! Any depositions outside this maximum are prohibited unless discussed first with the''' [[Brian Lingg|Tool Supervisor]]. |
|||
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 1)=== |
|||
*Recipe name: '''''CH3-TMA+H2O-<u>300C</u>''''' ("Thermal") |
|||
**300°C Dep., Thermal Water reaction |
|||
**This is considered the standard recipe for ALD |
|||
**TEMP = 300C, Al<sub>2</sub>O<sub>3</sub> deposition rate=1.3376 A/cyc |
|||
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1 A/cyc |
|||
**Recipe variations: ''TBD'' |
|||
===Pt deposition (ALD CHAMBER 1)=== |
|||
*Recipe name: '''''Ch1_TMCpPt+O3-300C''''' |
|||
**Pt deposition rate ~ 0.5-0.6 A/cyc |
|||
**Conductivity data: (to be added) |
|||
**recipe utilizes the ozone generator which must be first set to the following conditions: |
|||
***O<sub>2</sub> flow = 250sccm |
|||
***O<sub>3</sub> concentration = 15 wt% |
|||
**300°C deposition |
|||
*Recipe name: '''''CH1-TMCpPt+250W/O*-300C''''' |
|||
**Uses Oxygen plasma |
|||
**300°C deposition |
|||
===Ru deposition (ALD CHAMBER 1)=== |
|||
*Recipe name: '''''Ch1_Ex03Ru[HPbub]+O2-300C''''' |
|||
*Ru deposition rate ~ 0.6-0.7A/cyc. |
|||
*Conductivity data: (to be added) |
|||
*300°C, O2 gas reaction |
|||
===SiO{{sub|2}} deposition (ALD CHAMBER 1)=== |
|||
*Recipe name: '''''CH1-BDEAS-O*/300W-TEMP''''' |
|||
**Note that this recipe takes advantage of the higher-pressure range available in ch1 => faster than the lower pressure recipe available in ch3 |
|||
**SiO<sub>2</sub> deposition rate ~ 1-1.1 A/cyc |
|||
**TEMP = 300C (std), 250C, 230C, 200C, 150C, 120C |
|||
**Etch rate (BHF:DI=1:100)~7.46nm/min |
|||
*Recipe name: '''''CH1-BDEAS-O*/300W[LoP]-TEMP''''' |
|||
**replicates the (lower pressure) deposition conditions in ch3 for those that need it |
|||
**SiO<sub>2</sub> deposition rate ~ 0.9-1 A/cyc |
|||
**TEMP = 300C (std), 200C, 120C |
|||
**Etch rate (BHF:DI=1:100)~7.46nm/min |
|||
===ZnO Deposition (ALD Chamber 1)=== |
|||
''Conductive film.'' |
|||
*Recipe name: '''''Ch1_DEZ+H2O-200C''''' |
|||
*ZnO deposition rate ≈ 1.6 A/cycle |
|||
*resistivity ≈ ''TBA'' |
|||
*200°C Deposition, Water reaction |
|||
===ZnO:Al deposition (ALD CHAMBER 1)=== |
|||
''Al-Doped ZnO for variable resisitivity.'' |
|||
*Recipe name: '''''Ch1_DEZ/TMA+H2O-200C''''' |
|||
**''The recipe has TWO nested loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.'' |
|||
*Al dose fraction = 5% for lowest resistivity (loops: 1 TMA=Al loop per 19 DEX=Zn loops) |
|||
*ZnO deposition rate ~ 1.7A/cyc |
|||
*resistivity ~ 4200uOhm.cm (390A film) |
|||
==Oxford FlexAL Chamber #3: Dielectrics== |
|||
Unlike Chamber 1, Chamber 3 is restricted to a lower pressure range below 240 mTorr for all deposition steps. |
|||
'''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.) |
|||
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)=== |
|||
*Recipe name: '''''CH3-TMA+H2O-<u>TEMP</u>''''' ("Thermal") |
|||
**The proto-typical ALD recipe developed back in the 70's exhibiting perfect Lewis acid/base self-limiting surface reactions! |
|||
**Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1.1-1.2 A/cyc |
|||
**TEMP = 300C (std), 250C, 200C, 150C, 120C |
|||
**TEMP = 300C, Al<sub>2</sub>O<sub>3</sub> deposition rate=1.1973 A/cyc |
|||
**TEMP = 200C, Al<sub>2</sub>O<sub>3</sub> deposition rate=1.1631 A/cyc |
|||
**TEMP = 150C, Al<sub>2</sub>O<sub>3</sub> deposition rate=1.0852 A/cyc |
|||
*Recipe Name: '''''CH3-TMA+250W/O*-TEMP''''' ("Plasma") |
|||
**Activated O* Plasma reaction instead of H2O => non-thermal |
|||
**Lower carbon content |
|||
**Approx. <u>1.5–2x faster deposition rate</u> than thermal. |
|||
**TEMP= 300°C (std.), 200°C, 120°C |
|||
** |
|||
*Recipe Name: '''''CH3-TMA+O3/200mT-300C''''' ("Ozone") |
|||
**Similar dep. rate |
|||
**Ozone (O<sub>3</sub>) reactant, experimental |
|||
**Requires Ozone generator to be turned on - refer to notes above about the O3 generator. Need to consult with tool supervisor before first run! |
|||
===AlN deposition (ALD CHAMBER 3)=== |
|||
*Recipe name: '''''CH3-TMA+500W/N*-TEMP''''' |
|||
**AlN deposition rate ~ t.b.d. |
|||
**Recipe utilizes a N* plasma @ 100W, 20mTorr pressure. |
|||
**TEMP= 300°C Dep. (std.), 200*C, 120°C |
|||
** |
|||
*Recipe name: '''''CH3-TMA+100W/N*-300C''''' |
|||
**a cleaning/passivation process for III/V semiconductor surfaces prior to dielectric (gate) deposition |
|||
**Recipe utilizes a N* plasma @ 100W, 20mTorr pressure. |
|||
**Temperature Variations: 300°C Dep. (std.), 200*C, 120°C |
|||
** |
|||
===HfO{{sub|2}} deposition (ALD CHAMBER 3)=== |
|||
*Recipe name: '''''CH3-TEMAH+H2O-TEMP''''' ("Thermal") |
|||
**HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc, n[632nm]~2.0-2.1 |
|||
**Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
|||
**TEMP= 300°C (std.), 250°C, 200°C, 150°C, 120°C |
|||
*Recipe name: '''''CH3-TEMAH+250W/O*-300C''''' ("Plasma") |
|||
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
|||
** |
|||
*Recipe name: '''''CH3-TEMAH+O3/100mT-300C''''' ("Ozone") |
|||
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
|||
**Requires Ozone generator to be turned on - ask supervisor |
|||
===SiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
|||
*Recipe name: '''''CH3-BDEAS+300W/O*-<u>TEMP</u>''''' ("Plasma") |
|||
**SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc |
|||
**Recipe utilizes an O* plasma @ 40sccm O2, 300W ICP, 10mTorr pressure, |
|||
**TEMP = <u>300°C</u> (std.), 250°C, 230°C, 220°C, 200°C, 150°C, 120°C |
|||
**TEMP = <u>300°C,</u> dep. rate=1.2333 A/cyc |
|||
*Recipe name: '''''CH3-BDEAS+O3-300C''''' ("Ozone") |
|||
**Uses Ozone (O<sub>3</sub>) for reactant instead of O* plasma - still under development! |
|||
**Requires Ozone generator to be turned on - refer to notes above about the O3 generator. Need to consult with tool supervisor before first run! |
|||
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)=== |
|||
*Recipe name: '''''CH3-TEMAZ+H2O-<u>300C</u>''''' ("Thermal") |
|||
**ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
|||
**Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above. |
|||
**Temperature variations: <u>300°C</u> (std.), 200°C |
|||
*Recipe name: '''''CH3-TEMAZ+250W/O*-300C''''' ("Plasma") |
|||
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
|||
*Recipe name: '''''CH3-TEMAZ+O3/100mT-300C''''' ("Ozone") |
|||
**Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
|||
**Requires Ozone generator to be turned on - ask supervisor |
|||
===TiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
|||
*Recipe name: '''''CH3-TDMAT+H2O-300C''''' ("Thermal") |
|||
**TiO<sub>2</sub> deposition rate ~ 0.6A/cyc |
|||
**Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
|||
**Temperature variations: 300°C (std.), 200°C, 120*C |
|||
*Recipe name: '''''CH3-TDMAT+250W/O*-300C''''' ("Plasma") |
|||
**Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
|||
===TiN deposition (ALD CHAMBER 3)=== |
|||
*Recipe name: '''''CH3-TDMAT+400W/12N*/4H*-300C''''' |
|||
**TiN deposition rate ~ 0.7A/cyc |
|||
**Conductivity data: (to be added) |
|||
**Uses Plasma of N2 & H2 gases. |
|||
**Temperatures: 300°C (std.), 200°C |
|||
*Recipe name: '''''CH3-TDMAT+100W/N*-300C''''' |
|||
**Uses Plasma of N2 only |
|||
**Temperatures: 300°C (std.), 200°C |
|||
*Recipe name: '''''CH3-TDMAT+100W/NH3*-300C''''' |
|||
**Uses Plasma of NH<sub>3</sub> only |
|||
**Temperatures: 300°C (std.), 200°C |
|||
===Historical Data (ALD Chamber 3)=== |
|||
*[[Tbd|2021 ALD Al2O3 (H2O, 300°C) Historical Data]] |
|||
Latest revision as of 22:43, 21 May 2026
Back to Vacuum Deposition Recipes.
Atomic Layer Deposition (Oxford FlexAL)
Atomic Layer Deposition (aka ALD) - what is it?
Atomic layer deposition (ALD) utilizes sequential exposure cycles of 2 gaseous precursors to a substrate surface. Each half-cycle exposes one of the precursors to the substrate (and in the absence of the other) to ensure a "saturated" coverage on the surface. The saturation in exposure within each half-cycle leads to the self-limiting reaction behavior which defines an ALD process from other deposition techniques. With this in place, the deposition can proceed layer-by-layer with cycling and will result in uniform conformal growth over different substrate topographies.
In most standard process, one half-cycle utilizes an organometallic precursor to deposit the metal of interest. The other half-cycle utilizes a counter-reactant to either oxidize or nitridize this metal to form the oxide or nitride film required.
By nature of the deposition process, the reactions are slow. Hence, users are restricted to 30 nm maximum thickness for all films when using the tool. Any deviations from this requirement needs special permission (contact Tool Supervisor if needed).
Process Options
Thermal ALD
In all ALD processes used in our lab, the organometallic half-cycle is always thermal, i.e., the precursor is exposed to the substrate as a vapor. In a fully thermal ALD process, the counter reactant half-cycle also utilizes gas exposure to the substrate. Because the intact molecules are less reactive than activated gases from a plasma, thermal ALD can be on the slower side. One advantage however is this lower reactivity means that the substrate itself can remain inert to the deposition process.
Activated ALD
Plasma
O* or N* in the recipe title means Oxygen or Nitrogen plasma, derived from flowing O2 or N2 gases through the ICP tube at the top of the chamber, respectively.
The plasma processes on this tool will run considerably faster than purely thermal processes, because the ions/radicals formed are significantly more reactive (which can be a drawback if depositing on a sensitive substrate). Note that the O* plasma can also reduce carbon contaminants from the organic precursors when forming oxide films. When growing nitride films, H2 is often added to the nitride-plasma gases to generate H* ions/radicals which can assist with the removal of C within the film.
Ozone
O3 in the recipe title refers to an oxidation reaction that uses an external Ozone generator for oxide growth (InUSA, Series 5000). Ozone is a more reactive form of oxygen than O2 that can be used to generate oxide films in a more thermal manner than plasma (which can sometimes be too aggressive).
Note that the generator must first be turned on prior to running any ozone-based recipe. Clicking on the O3 Generator icon on the tool desktop will open the control window. Both the O2 flow and the O3 concentration should be set to the defaults of 250 sccm and 19 wt% in the field settings. Clicking on the "Start Generator" button will start the ozone generator running. Wait for about 5 minutes for the system to stabilize. When done, always be sure to click on the "Stop Generator" button to turn off the generator and stop the O2 flow - it is very important not to forget to do this as the source could be burned out and/or the O2 bottle supplying the generator could be depleted if it runs too long! O2 will remain flowing for an additional minute to flush out any residual O3. Once that is completed, you can close the window. Check with supervisor for further details.
Chamber #1: Conductive Films
Chamber 1 utilizes a dual manometer system that allows higher pressures during deposition than chamber 3. For example, chamber 1 has an upper limit of 2000 mTorr whereas chamber 3 has an upper limit of only 240 mTorr. The higher pressures allow the use of less reactive organo-metallic precursors to effect ALD growth in a reasonable time-frame.
Maximum 30nm deposition thickness for all processes in chamber 1! Any depositions outside this maximum are prohibited unless discussed first with the Tool Supervisor.
Al2O3 deposition (ALD CHAMBER 1)
- Recipe name: CH3-TMA+H2O-300C ("Thermal")
- 300°C Dep., Thermal Water reaction
- This is considered the standard recipe for ALD
- TEMP = 300C, Al2O3 deposition rate=1.3376 A/cyc
- Al2O3 deposition rate ~ 1 A/cyc
- Recipe variations: TBD
Pt deposition (ALD CHAMBER 1)
- Recipe name: Ch1_TMCpPt+O3-300C
- Pt deposition rate ~ 0.5-0.6 A/cyc
- Conductivity data: (to be added)
- recipe utilizes the ozone generator which must be first set to the following conditions:
- O2 flow = 250sccm
- O3 concentration = 15 wt%
- 300°C deposition
- Recipe name: CH1-TMCpPt+250W/O*-300C
- Uses Oxygen plasma
- 300°C deposition
Ru deposition (ALD CHAMBER 1)
- Recipe name: Ch1_Ex03Ru[HPbub]+O2-300C
- Ru deposition rate ~ 0.6-0.7A/cyc.
- Conductivity data: (to be added)
- 300°C, O2 gas reaction
SiO2 deposition (ALD CHAMBER 1)
- Recipe name: CH1-BDEAS-O*/300W-TEMP
- Note that this recipe takes advantage of the higher-pressure range available in ch1 => faster than the lower pressure recipe available in ch3
- SiO2 deposition rate ~ 1-1.1 A/cyc
- TEMP = 300C (std), 250C, 230C, 200C, 150C, 120C
- Etch rate (BHF:DI=1:100)~7.46nm/min
- Recipe name: CH1-BDEAS-O*/300W[LoP]-TEMP
- replicates the (lower pressure) deposition conditions in ch3 for those that need it
- SiO2 deposition rate ~ 0.9-1 A/cyc
- TEMP = 300C (std), 200C, 120C
- Etch rate (BHF:DI=1:100)~7.46nm/min
ZnO Deposition (ALD Chamber 1)
Conductive film.
- Recipe name: Ch1_DEZ+H2O-200C
- ZnO deposition rate ≈ 1.6 A/cycle
- resistivity ≈ TBA
- 200°C Deposition, Water reaction
ZnO:Al deposition (ALD CHAMBER 1)
Al-Doped ZnO for variable resisitivity.
- Recipe name: Ch1_DEZ/TMA+H2O-200C
- The recipe has TWO nested loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.
- Al dose fraction = 5% for lowest resistivity (loops: 1 TMA=Al loop per 19 DEX=Zn loops)
- ZnO deposition rate ~ 1.7A/cyc
- resistivity ~ 4200uOhm.cm (390A film)
Oxford FlexAL Chamber #3: Dielectrics
Unlike Chamber 1, Chamber 3 is restricted to a lower pressure range below 240 mTorr for all deposition steps.
Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)
Al2O3 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TMA+H2O-TEMP ("Thermal")
- The proto-typical ALD recipe developed back in the 70's exhibiting perfect Lewis acid/base self-limiting surface reactions!
- Al2O3 deposition rate ~ 1.1-1.2 A/cyc
- TEMP = 300C (std), 250C, 200C, 150C, 120C
- TEMP = 300C, Al2O3 deposition rate=1.1973 A/cyc
- TEMP = 200C, Al2O3 deposition rate=1.1631 A/cyc
- TEMP = 150C, Al2O3 deposition rate=1.0852 A/cyc
- Recipe Name: CH3-TMA+250W/O*-TEMP ("Plasma")
- Activated O* Plasma reaction instead of H2O => non-thermal
- Lower carbon content
- Approx. 1.5–2x faster deposition rate than thermal.
- TEMP= 300°C (std.), 200°C, 120°C
- Recipe Name: CH3-TMA+O3/200mT-300C ("Ozone")
- Similar dep. rate
- Ozone (O3) reactant, experimental
- Requires Ozone generator to be turned on - refer to notes above about the O3 generator. Need to consult with tool supervisor before first run!
AlN deposition (ALD CHAMBER 3)
- Recipe name: CH3-TMA+500W/N*-TEMP
- AlN deposition rate ~ t.b.d.
- Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
- TEMP= 300°C Dep. (std.), 200*C, 120°C
- Recipe name: CH3-TMA+100W/N*-300C
- a cleaning/passivation process for III/V semiconductor surfaces prior to dielectric (gate) deposition
- Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
- Temperature Variations: 300°C Dep. (std.), 200*C, 120°C
HfO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TEMAH+H2O-TEMP ("Thermal")
- HfO2 deposition rate ~ 0.9-1.0A/cyc, n[632nm]~2.0-2.1
- Note: deposition shows significant parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
- TEMP= 300°C (std.), 250°C, 200°C, 150°C, 120°C
- Recipe name: CH3-TEMAH+250W/O*-300C ("Plasma")
- Uses Oxygen plasma reactant instead of H2O
- Recipe name: CH3-TEMAH+O3/100mT-300C ("Ozone")
- Uses Ozone (O3) for reactant instead of H2O
- Requires Ozone generator to be turned on - ask supervisor
SiO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-BDEAS+300W/O*-TEMP ("Plasma")
- SiO2 deposition rate ~ 0.7-0.8A/cyc
- Recipe utilizes an O* plasma @ 40sccm O2, 300W ICP, 10mTorr pressure,
- TEMP = 300°C (std.), 250°C, 230°C, 220°C, 200°C, 150°C, 120°C
- TEMP = 300°C, dep. rate=1.2333 A/cyc
- Recipe name: CH3-BDEAS+O3-300C ("Ozone")
- Uses Ozone (O3) for reactant instead of O* plasma - still under development!
- Requires Ozone generator to be turned on - refer to notes above about the O3 generator. Need to consult with tool supervisor before first run!
ZrO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TEMAZ+H2O-300C ("Thermal")
- ZrO2 deposition rate ~ 0.9-1.0A/cyc
- Not directly characterized since results are basically the same as the HfO2 process above.
- Temperature variations: 300°C (std.), 200°C
- Recipe name: CH3-TEMAZ+250W/O*-300C ("Plasma")
- Uses Oxygen plasma reactant instead of H2O
- Recipe name: CH3-TEMAZ+O3/100mT-300C ("Ozone")
- Uses Ozone (O3) for reactant instead of H2O
- Requires Ozone generator to be turned on - ask supervisor
TiO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAT+H2O-300C ("Thermal")
- TiO2 deposition rate ~ 0.6A/cyc
- Note: deposition shows parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
- Temperature variations: 300°C (std.), 200°C, 120*C
- Recipe name: CH3-TDMAT+250W/O*-300C ("Plasma")
- Uses Oxygen plasma reactant instead of H2O
TiN deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAT+400W/12N*/4H*-300C
- TiN deposition rate ~ 0.7A/cyc
- Conductivity data: (to be added)
- Uses Plasma of N2 & H2 gases.
- Temperatures: 300°C (std.), 200°C
- Recipe name: CH3-TDMAT+100W/N*-300C
- Uses Plasma of N2 only
- Temperatures: 300°C (std.), 200°C
- Recipe name: CH3-TDMAT+100W/NH3*-300C
- Uses Plasma of NH3 only
- Temperatures: 300°C (std.), 200°C