Thermal Evaporation Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
No edit summary
Biljana (talk | contribs)
 
(38 intermediate revisions by 2 users not shown)
Line 2: Line 2:


=[[Thermal Evaporator 1]]=
=[[Thermal Evaporator 1]]=

⚫
== Materials Table ==
==Materials Table==


{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
|-
|-
! colspan=8 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table</div>
! colspan=8 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table for Thermal Evaporator #1</div>
|- bgcolor="#D0E7FF"
|- bgcolor="#D0E7FF"
! width="45" bgcolor="#D0E7FF" align="center" | '''Material'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Material'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Symbol'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Symbol'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Density, g/cm3'''
! width="95" bgcolor="#D0E7FF" align="center" | '''Density, g/cm3'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Z Ratio'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Z Ratio'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Tooling, %'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Tooling, %'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Current, Amp'''
! width="95" bgcolor="#D0E7FF" align="center" | '''Current, Amp'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Dep.rate, A/sec'''
! width="95" bgcolor="#D0E7FF" align="center" | '''Dep.rate, A/sec'''
! width="100" bgcolor="#D0E7FF" align="center" | '''Comments'''
! width="95" bgcolor="#D0E7FF" align="center" | '''Comments'''
|-
|-
|Aluminum
|Aluminum
Line 28: Line 29:
|Chromium
|Chromium
|Cr
|Cr
| 7.20
|7.20
| 28.95
|28.95
|95
|95
|85
|85
Line 179: Line 180:
|
|
|-
|-
|Strontium Fluoride
|StrontiumFluoride
|SrF<sub>2
|SrF<sub>2
|4.28
|4.28
|12.15
|12.15
Line 198: Line 199:
|-
|-
|ITO(IndiumTinOxide)
|ITO(IndiumTinOxide)
|In<sub>2</sub>O<sub>3</sub> - SnO<sub>2</sub>
|In<sub>2</sub>O<sub>3</sub> - SnO<sub>2
|6.43-7.14
|6.43-7.14
|0.841
|0.841
Line 206: Line 207:
|
|
|-
|-
|Permalloy
|Permalloy
|Ni<sub>0.1</sub>Fe<sub>0.2
|Ni<sub>0.1</sub>Fe<sub>0.2</sub>
|8.7
|8.7
|26.40
|26.40
Line 214: Line 215:
|0.1
|0.1
|
|
|-
|}


=[[Thermal Evaporator 2]]=
=[[Thermal Evaporator 2]]=

⚫
= Materials Table =
⚫
== Materials Table ==


{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
{| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" class="collapsible collapsed wikitable"
|-
|-
! colspan=6 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table</div>
! colspan=6 width=1300 height=35 bgcolor="#D0E7FF" align="center"|<div style="font-size: 150%;">Materials Table for Thermal Evaporator #2</div>
|- bgcolor="#D0E7FF"
|- bgcolor="#D0E7FF"
! width="45" bgcolor="#D0E7FF" align="center" | '''Material'''
! width="45" bgcolor="#D0E7FF" align="center" | '''Material'''
Line 354: Line 356:
|0.841
|0.841
|120
|120
|Used often
|Used often, tooling factor needs adjustment
|-
|-
|Indium antimonide
|Indium antimonide
Line 570: Line 572:
|7.30
|7.30
|0.724
|0.724
|
|197
|Program #9, Tooling factor=200%, cold fixture
|Used often
|-
|-
|Titanium
|Titanium
Line 642: Line 644:
|
|
|
|
|-
|}

== In Deposition (Thermal Evaporator 2) ==
*[[Media:Thermal evaporator 2-new Sheet1.pdf|Indium evaporation Data]]

Latest revision as of 21:27, 19 June 2025

Back to Vacuum Deposition Recipes.

Thermal Evaporator 1

Materials Table

Thermal Evaporator 2

Materials Table

In Deposition (Thermal Evaporator 2)