Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer): Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
moved SEM images to table, changed "File:" link --> Direct link to file
Ningcao (talk | contribs)
add one SEM pic
Line 15: Line 15:
|0.74
|0.74
|77.9
|77.9
|[https://www.nanotech.ucsb.edu/wiki/index.php/File:SiO2_Etch_using_ICP2_with_O2.pdf]
|
|-
|-
|1/28/2019
|1/28/2019

Revision as of 17:22, 31 January 2019

ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
10/5/2018 SiO2#01 95.2 0.74 77.9 [1]
1/28/2019 I21902 92.1 0.77 [2]