*[[media:PECVD1-SiON-Recipe.pdf|SiO<sub>x</sub>N<sub>y</sub> Deposition Recipes - Varying N/O Ratio]] |
*[[media:PECVD1-SiON-Recipe.pdf|SiO<sub>x</sub>N<sub>y</sub> Deposition Recipes - Varying N/O Ratio]] |
||
*[[media:PECVD1-SiON-Plot.pdf|SiO<sub>x</sub>N<sub>y</sub> Stress/Index vs. O/N Ratio]] |
*[[media:PECVD1-SiON-Plot.pdf|SiO<sub>x</sub>N<sub>y</sub> Stress/Index vs. O/N Ratio]] |
||
*[[media:PECVD1- |
*[[media:PECVD1-LS SION recipe 2014.pdf|SiO<sub>x</sub>N<sub>y</sub> Recipe]] |
||
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data November 2014] |
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data November 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub> 3000A Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub> 3000A Thickness uniformity 2014] |
||
Revision as of 23:22, 3 December 2014
PECVD 1 (PlasmaTherm 790)
SiN deposition (PECVD #1)
- SiN Standard Recipe
- SiN Data November 2014
- SiN 1000A Thickness uniformity 2014
- Low Stress Si3N4 - Variable Stress Recipes
- Low Stress Si3N4 - Variable Stress Plot
- Deposition rate~11.23nm/min (users must calibrate this prior to critical deps)
- HF e.r.~89nm/min
- Stress~450MPa
- Refractive Index~1.942
SiO2 deposition (PECVD #1)
- Deposition rate~35.52nm/min (users must calibrate this prior to critical deps)
- HF e.r.~645nm/min
- Stress~-408MPa
- Refractive Index~1.461
SiOxNy deposition (PECVD #1)
- SiOxNy Deposition Recipes - Varying N/O Ratio
- SiOxNy Stress/Index vs. O/N Ratio
- SiOxNy Recipe
- SiOxNy Data November 2014
- SiOxNy 3000A Thickness uniformity 2014
- Deposition rate~14.99nm/min (users must calibrate this prior to critical deps)
- HF e.r.~417nm/min
- Stress~133MPa
- Refractive Index~1.714