== SiN deposition (PECVD #1) ==
== SiN deposition (PECVD #1) ==
*[[media:PECVD1-SiN-standard recipe 2014.pdf|SiN Standard Recipe]]
*[[media:PECVD1-SiN-standard recipe 2014.pdf|SiN Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN Data November 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN Data December 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 1000A Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 1000A Thickness uniformity 2014]
<!-- Placeholders - Not uploaded yet-->
<!-- Placeholders - Not uploaded yet-->

Revision as of 23:42, 3 December 2014

PECVD 1 (PlasmaTherm 790)

SiN deposition (PECVD #1)

  • Deposition rate~11.23nm/min (users must calibrate this prior to critical deps)
  • HF e.r.~89nm/min
  • Stress~450MPa
  • Refractive Index~1.942

SiO2 deposition (PECVD #1)

  • Deposition rate~35.52nm/min (users must calibrate this prior to critical deps)
  • HF e.r.~645nm/min
  • Stress~-408MPa
  • Refractive Index~1.461

SiOxNy deposition (PECVD #1)

  • Deposition rate~14.99nm/min (users must calibrate this prior to critical deps)
  • HF e.r.~417nm/min
  • Stress~133MPa
  • Refractive Index~1.714