Dry Etching Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
link to ICP2 Ru etch
m fix ICP1 GaAs link
Line 2: Line 2:
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
! colspan="17" width="725" height="45" | <div style="font-size: 150%;">Dry Etching Recipes</div>
! colspan="17" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
|- bgcolor="#d0e7ff"
|- bgcolor="#d0e7ff"
| <!-- INTENTIONALLY LEFT BLANK -->
|<!-- INTENTIONALLY LEFT BLANK -->
! colspan="4" width="300" height="35" align="center" bgcolor="#d0e7ff" | '''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="4" width="300" height="35" align="center" bgcolor="#d0e7ff" |'''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="4" align="center" bgcolor="#d0e7ff" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="4" align="center" bgcolor="#d0e7ff" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="3" align="center" bgcolor="#d0e7ff" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
! colspan="3" align="center" bgcolor="#d0e7ff" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
|-
|-
! width="65" align="center" bgcolor="#d0e7ff" | '''Material'''
! width="65" align="center" bgcolor="#d0e7ff" |'''Material'''
| width="65" bgcolor="#daf1ff" | [[RIE 1 (Custom)|RIE 1<br>(Retired)]]
| width="65" bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
| width="65" bgcolor="#daf1ff" | [[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| width="65" bgcolor="#daf1ff" | [[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| width="100" bgcolor="#daf1ff" | [[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| width="100" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| width="100" bgcolor="#daf1ff" | [[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| width="100" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| width="100" bgcolor="#daf1ff" | [https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)]
| width="100" bgcolor="#daf1ff" |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)]
| width="120" bgcolor="#daf1ff" | [[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]]
| width="120" bgcolor="#daf1ff" | [[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]]
| width="85" bgcolor="#daf1ff" | [[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| width="85" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| width="85" bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| width="95" bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| width="95" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| width="85" bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| width="85" bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| width="85" bgcolor="#daf1ff" | [[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| width="85" bgcolor="#daf1ff" | [[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| width="85" bgcolor="#daf1ff" | [[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Ag
! align="center" bgcolor="#d0e7ff" |Ag
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Al
! align="center" bgcolor="#d0e7ff" |Al
|
|
|
|
|
|
| [[RIE Etching Recipes|A]]
|[[RIE Etching Recipes|A]]
|
|
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|Al Etch (Panasonic 2)}}
|
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|Al Etch (Panasonic 1)}}
| {{rl|ICP Etching Recipes|Al Etch (Panasonic 2)}}
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Au
! align="center" bgcolor="#d0e7ff" |Au
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|[https://www.nanotech.ucsb.edu/wiki/index.php/Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29 A]
|[https://www.nanotech.ucsb.edu/wiki/index.php/Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29 A]
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Cr
! align="center" bgcolor="#d0e7ff" |Cr
|
|
|
|
|
|
| A
|A
|
|
|{{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
|A
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|Cr Etch (Panasonic 1)}}
| A
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Cu
! align="center" bgcolor="#d0e7ff" |Cu
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Ge
! align="center" bgcolor="#d0e7ff" |Ge
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
| A
|
|
|
|
|A
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Mo
! align="center" bgcolor="#d0e7ff" |Mo
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Ni
! align="center" bgcolor="#d0e7ff" |Ni
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
|-
! align="center" bgcolor="#d0e7ff" | Pt
! align="center" bgcolor="#d0e7ff" |Pt
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|
|
|
|
|
|
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
|-
! align="center" bgcolor="#d0e7ff" | Ru
! align="center" bgcolor="#d0e7ff" |Ru
|
|
|
|
|
|
|
|
|
|
|A
|{{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}}
|
|
|
|
|
|
|
|
| A
| {{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}}
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Si
! align="center" bgcolor="#d0e7ff" |Si
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}}
|{{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}}
| {{Rl|ICP Etching Recipes|Si Etching}}
|{{Rl|ICP Etching Recipes|Si Etching}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|
| {{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Ta
! align="center" bgcolor="#d0e7ff" |Ta
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Ti
! align="center" bgcolor="#d0e7ff" |Ti
|
|
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
|A
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|Ti Etch (Panasonic 1)}}
| A
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Al<sub>2</sub>O<sub>3</sub>
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3</sub>
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
|
|
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
|A
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|Sapphire Etch (Panasonic 1)}}
| A
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | AlGaAs
! align="center" bgcolor="#d0e7ff" |AlGaAs
|
|
|
|
|
|
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
|
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
|
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | AlGaN
! align="center" bgcolor="#d0e7ff" |AlGaN
|
|
|
|
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | AlN
! align="center" bgcolor="#d0e7ff" |AlN
|
|
|
|
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | CdZnTe
! align="center" bgcolor="#d0e7ff" |CdZnTe
|
|
| {{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | GaAs
! align="center" bgcolor="#d0e7ff" |GaAs
|
|
|
| {{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|
|
|
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}}
|{{rl|RIE Etching Recipes|AlGaAs\GaAs Etching (RIE 5)}}
|
|
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}}
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}}
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}}
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | GaN
! align="center" bgcolor="#d0e7ff" |GaN
|
|
|
|
|
|
| {{rl|RIE Etching Recipes|GaN Etching (RIE 5)}}
|{{rl|RIE Etching Recipes|GaN Etching (RIE 5)}}
|
|
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
|
| {{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | GaSb
! align="center" bgcolor="#d0e7ff" |GaSb
|
|
|
|
|
|
|
|
|
|
|
|A
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
|
|
|
|
|
|
|
| A
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | HfO<sub>2</sub>
! align="center" bgcolor="#d0e7ff" |HfO<sub>2</sub>
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | InGaAlAs
! align="center" bgcolor="#d0e7ff" |InGaAlAs
|
|
| {{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | InGaAsP
! align="center" bgcolor="#d0e7ff" |InGaAsP
|
|
| {{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | InP
! align="center" bgcolor="#d0e7ff" |InP
|
|
| {{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
|
|
|
|
|
|
|A
|A
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
| A
| A
| {{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | ITO
! align="center" bgcolor="#d0e7ff" |ITO
|
|
| {{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
!Photoresist
!Photoresist
Line 533: Line 533:
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | SiC
! align="center" bgcolor="#d0e7ff" |SiC
|
|
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
|A
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|SiC Etch (Panasonic 1)}}
| A
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | SiN
! align="center" bgcolor="#d0e7ff" |SiN
|
|
|
|
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
|
|
|
|
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}}
|
|A
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
| {{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}}
|
| A
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | SiO<sub>2</sub>
! align="center" bgcolor="#d0e7ff" |SiO<sub>2</sub>
|
|
| {{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
|
|
|
| A
| {{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
| {{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
|
|
|
|
|
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
|
|
|
|
| {{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
|A
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
|
|
|
|
|
|
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | SiOxNy
! align="center" bgcolor="#d0e7ff" |SiOxNy
|
|
|
|
|
|
|
|
|
|
|
|
|A
|A
|A
|A
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | Ta<sub>2</sub>O<sub>5</sub>
! align="center" bgcolor="#d0e7ff" |Ta<sub>2</sub>O<sub>5</sub>
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A]
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A]
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | TiN
! align="center" bgcolor="#d0e7ff" |TiN
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | TiO<sub>2</sub>
! align="center" bgcolor="#d0e7ff" |TiO<sub>2</sub>
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | W-TiW
! align="center" bgcolor="#d0e7ff" |W-TiW
|
|
|
|
|
|
|
|
|
|
|{{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
|A
|
|
|
|
|
|
|
|
| {{rl|ICP Etching Recipes|W-TiW Etch (Panasonic 1)}}
| A
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" | ZnO<sub>2</sub>
! align="center" bgcolor="#d0e7ff" |ZnO<sub>2</sub>
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | ZnS
! align="center" bgcolor="#d0e7ff" |ZnS
|
|
| {{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | ZnSe
! align="center" bgcolor="#d0e7ff" |ZnSe
|
|
| {{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | ZrO<sub>2</sub>
! align="center" bgcolor="#d0e7ff" |ZrO<sub>2</sub>
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
|-
! align="center" bgcolor="#d0e7ff" | '''Material'''
! align="center" bgcolor="#d0e7ff" |'''Material'''
| bgcolor="#daf1ff" | [[RIE 1 (Custom)|RIE 1<br>(Retired)]]
| bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
| bgcolor="#daf1ff" | [[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
| bgcolor="#daf1ff" | [[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
| bgcolor="#daf1ff" | [[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" | [[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| bgcolor="#daf1ff" | [[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|SLR Fluorine ICP (PlasmaTherm)]]
| bgcolor="#daf1ff" |[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|SLR Fluorine ICP (PlasmaTherm)]]
| bgcolor="#daf1ff" | [[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic E626I)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic E626I)]]
| bgcolor="#daf1ff" | [[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic E640)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic E640)]]
| bgcolor="#daf1ff" | [[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
| bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
| bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" | [[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
| bgcolor="#daf1ff" | [[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
| bgcolor="#daf1ff" | [[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
| bgcolor="#daf1ff" | [[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
|}
|}



Revision as of 20:33, 27 August 2019

  • R = Recipe is available. Clicking this link will take you to the recipe.
  • A = Material is available for use, but no recipes are provided.
Dry Etching Recipes
RIE Etching ICP Etching Oxygen Plasma Systems Other Dry Etchers
Material RIE 1
(Retired)
RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
SLR Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic 1)
ICP Etch 2
(Panasonic 2)
ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)
Ag
Al A R1 R1
Au A
Cr A R1 A
Cu
Ge A
Mo
Ni R1
Pt R1
Ru A R1
Si R1 R1 R1
Ta
Ti R1 A
Al2O3 R
Al2O3 (Sapphire) R1 A
AlGaAs R1 R1 GaAs-AlGaAs Etch (Unaxis VLR)
AlGaN R1
AlN R1
CdZnTe R1
GaAs R1 R1 R1 GaAs-AlGaAs Etch (Unaxis VLR)
GaN R1 R1 R1
GaSb A GaSb Etch Unaxis VLR)
HfO2
InGaAlAs InP-InGaAsP-InGaAlAs Etching (RIE 2) InP-InGaAs-InAlAs Etch (Unaxis VLR)
InGaAsP InP-InGaAsP-InGaAlAs Etching (RIE 2) InP-InGaAs-InAlAs Etch (Unaxis VLR)
InP InP-InGaAsP-InGaAlAs Etching (RIE 2) A A InP-InGaAs-InAlAs Etch (Unaxis VLR)
ITO R1
Photoresist

& ARC

A R R R A A
SiC R1 A
SiN SiNx Etching (RIE 3) R1 R1 A
SiO2 SiO2 Etching (RIE 3) A R1 R1 R1
SiOxNy A A
Ta2O5 A
TiN
TiO2
W-TiW R1 A
ZnO2
ZnS R1
ZnSe R1
ZrO2
Material RIE 1
(Retired)
RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
SLR Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)