Test Data of etching SiO2 with CHF3/CF4: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
pasted link to alternate etch data
Line 86: Line 86:
|After etching diamond sample for 1 hour using Cl2/Ar
|After etching diamond sample for 1 hour using Cl2/Ar
|[https://wiki.nanotech.ucsb.edu/w/images/2/26/I2210508.pdf]
|[https://wiki.nanotech.ucsb.edu/w/images/2/26/I2210508.pdf]
|}
|}<br />
⚫
===Alternate Data (not updated)===
''We stopped taking data for the following table in 2019, use the above data instead.''


⚫
*[[Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer)|Test Data of etching SiO2 with CHF3/CF4/O2]]
⚫
=== Alternate Data (not updated since 2019) ===

⚫
* [[Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer)|Test Data of etching SiO2 with CHF3/CF4/O2]]

Revision as of 18:13, 4 January 2022

ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
10/5/2018 SiO2#02 160 1.2 82.1 [1]
1/28/2019 I21901 146 1.23 [2]
3/6/2019 I21904 151 1.23 85.6 [3]
7/18/2019 I21905 162 1.37 [4]
1/16/2020 I22001 149 1.21 [5]
8/9/2020 I22002 102 0.86 caused by air leaking to CHF3 channel [6]
1/7/2021 I22101 144 1.20 [7]
5/19/2021 I22102 163 1.11 Etch time=130 sec [8]
7/21/2021 I22103 134 1.09 Investigating reports of low etch rate [9]
8/9/2021 I22104 147 1.06 Before etching diamond sample for 1 hour using Cl2/Ar [10]
8/9/2021 I22105 140 0.97 After etching diamond sample for 1 hour using Cl2/Ar [11]


Alternate Data (not updated)

We stopped taking data for the following table in 2019, use the above data instead.