Dry Etching Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
smaller fonts to make table more obvious
added LiNbO3, SU8, BCB
Line 4: Line 4:
===Dry Etching Tools/Materials Table===
===Dry Etching Tools/Materials Table===


* <small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small>
*<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small>
* <small>'''A''': ''Material is available for use, but no recipes are provided.''</small>
*<small>'''A''': ''Material is available for use, but no recipes are provided.''</small>


{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
Line 327: Line 327:
|
|
|
|
|
|A
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|
|
Line 415: Line 415:
|
|
|A
|A
⚫
|-
!BCB
⚫
|
|
|
|
|
|A
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |CdZnTe
! bgcolor="#d0e7ff" align="center" |CdZnTe
Line 474: Line 493:
|- bgcolor="#ffffff"
|- bgcolor="#ffffff"
! bgcolor="#d0e7ff" align="center" |GaSb
! bgcolor="#d0e7ff" align="center" |GaSb
⚫
|
|
|
|
|
Line 481: Line 499:
|
|
|A
|A
|
|A
|A
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
|
|
Line 570: Line 589:
! bgcolor="#d0e7ff" align="center" |ITO
! bgcolor="#d0e7ff" align="center" |ITO
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|A
|-
!LiNbO3
|
|
|
|
|
Line 598: Line 636:
|
|
|
|
|R
|A
|A
|A
|R
⚫
|A
|
|
|
|
Line 701: Line 739:
|
|
|A
|A
|-
!SU8
|
|
|
|
|
|A
|
|
|
|
|
|
|
|
|
|
|
|- bgcolor="#eeffff"
|- bgcolor="#eeffff"
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
Line 708: Line 765:
|
|
|
|
|
|A
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A]
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A]
|
|

Revision as of 22:59, 7 July 2022

Process Control Data

See linked page for process control data (dep rate/stress etc. over time), for a selection of often-used thin-film depositions.

Dry Etching Tools/Materials Table

  • R: Recipe is available. Clicking this link will take you to the recipe.
  • A: Material is available for use, but no recipes are provided.
Dry Etching Recipes
RIE Etching ICP Etching Oxygen Plasma Systems Other Dry Etchers
Material RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
Oxford ICP (PlasmaPro 100) ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)
Ag A
Al A R1 R1 A
Au R1
Cr A R1 A A
Cu A
Ge A A A A
Mo A
Nb A A
Ni R1
Os A A
Pt R1
Ru A R1 A
Si R1 R1 A R1 A
Ta A A A
Ti R1 A A
Al2O3 A R A
Al2O3 (Sapphire) R1 A A
AlGaAs R1 R1 R GaAs-AlGaAs Etch (Unaxis VLR) A
AlGaN R R1 A
AlN R1 A
BCB A
CdZnTe R1 A
GaAs R1 R1 R1 R GaAs-AlGaAs Etch (Unaxis VLR) A
GaN R1 R1 A R R1 A
GaSb A A A GaSb Etch Unaxis VLR) A
HfO2 A
InGaAlAs InP-InGaAsP-InGaAlAs Etching (RIE 2) A InP-InGaAs-InAlAs Etch (Unaxis VLR) A
InGaAsP InP-InGaAsP-InGaAlAs Etching (RIE 2) R InP-InGaAs-InAlAs Etch (Unaxis VLR) A
InP InP-InGaAsP-InGaAlAs Etching (RIE 2) A A R InP-InGaAs-InAlAs Etch (Unaxis VLR) R1
ITO R1 A
LiNbO3 A
Photoresist

& ARC

A R R R R R A R A
Ru A R
SiC R1 A A
SiN SiNx Etching (RIE 3) A R1 R1 A A
SiO2 SiO2 Etching (RIE 3) R1 R1 R1 R1 A
SiOxNy A A A
SU8 A
Ta2O5 A A A
TiN A
TiO2 A
W-TiW R1 A A
ZnO2 A
ZnS R1 A
ZnSe R1 A
ZrO2 A
Material RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
Oxford ICP (PlasmaPro 100) ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)